Skip to main content

RE: Atención valide origen![MW:30159] Fwd: Nozzle crack propagation

Hello

Initially, in my opinion there is not SS flange, but you can check, by using the devise for that.

This corrosion evidence indicate that the material isn´t SS.

According to the picture, the crack is far away from the weld. We can suppose that that the failure in not associated to the welding process, but the material quality.

                                                                                                                                                                                               

 

Hernán Castillo Mier

Ingeniero Senior Confiabilidad e Integridad

FACILITADOR AUTORIDAD TÉCNICA EQUIPO ESTÁTICO

INSPECTOR AUTORIZADO

API 510 (33119)

Avantel: 8*1571

Teléfono: 668-2396

 

De: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] En nombre de Chiranjeevi A
Enviado el: miércoles, 16 de octubre de 2019 3:32 PM
Para: materials-welding@googlegroups.com
Asunto: Atención valide origen![MW:30153] Fwd: Nozzle crack propagation

 

 

Dear All,

   Please find the attached snap, we found a crack circumferentially. The nozzle size is 6" and the material is SS.

 

  The following plant is under construction and the vessel erected around 1yr back. There is an argument that because of pipe loads that are not supported yet, it created tension and lead to crack.  Even I surprised that how a steel material started cracked like brittle for just for a few external loads. (This not the correct reason)

 

I clearly explained that any steel material that we design to be below the yield value. When the load beyond the ultimate limit it leads to fatigue and finally crack. This situation we can expect in operation if there is cyclic loading and the connected piping not supported properly. (which is an impossible situation).

 

 Finally, I suspect that 

 - the material of the nozzle is not SS. (Maybe zinc coated)

- (or) Because of  corrosion

- 

(or) during welding, it created a weaker section and started crack initiation for the external loads.

 

Experts kindly share your opinion and suggestions.

 

Thanks & Regards

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAN4%2Bm0wDkxeQNHY0mBcit_VfEDhKueRp%2BWnURJehau-%3DXz_sPA%40mail.gmail.com.

Este mensaje puede contener información de tipo personal, clasificada o reservada; si usted no es el destinario, por favor, hacer caso omiso de su contenido y abstenerse de compartirlo, reenviarlo o copiarlo. Si recibe este mensaje por error, agradecemos informarlo inmediatamente al remitente y borrarlo permanentemente de su cuenta. Si usted está autorizado para recibir la información de tipo personal, se le recuerda que esta información debe ser manejada con la finalidad con la que ha sido solicitada y en virtud de la normativa que habilita el acceso a la misma. Así mismo, deberá ser usada bajo los parámetros de la ley 1581 de 2012 de protección de datos personales y la normativa que la desarrolla, siendo responsabilidad del área receptora del cumplimiento de la citada normativa de protección de datos personales. CONFIDENTIALITY NOTICE: This electronic transmission (including any files attached hereto) (this "Communication") contains information that is or may be legally privileged, confidential, and exempt from disclosure without our express permission in advance. The information is intended only for the use of the individual or entity named above. If the reader of this message is not the intended recipient or any employee or agent responsible for delivering the message to the intended recipient, you are hereby notified that any disclosure, dissemination, copying, distribution, or the taking of any action in reliance on the contents of this electronic Communication is strictly prohibited. If you have received this Communication in error, please notify the sender immediately and destroy permanently the transmitted information in its entirety and do not disclose its contents to any other person. Para conocer la Declaración de Tratamiento de Datos Personales de Ecopetrol, favor consultarla en www.ecopetrol.com.co Responsabilidad Corporativa – Declaración de Tratamiento de Datos Personales.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...