Skip to main content

Re: [MW:27377] If a welder is qualified with SS (Stainless Steel) GTAW, He can weld CS Carbon steel GTAW?

Good morning everyone 

Sir you are write. 

For GTAW can not weld due to essential variables deletion of fas. 

Regards 
Anand gupta
Iocl  baroda


On Sun, 25 Feb 2018 at 8:38 AM, Amit Singh
<kshtriya.amit@gmail.com> wrote:
Removal of Gas Backing is essential variable that's why a SS GTAW qualified welder is not qualified for CS GTAW joints, however reverse can be true for GTAW procedure only
Regards, 
Amit Singh

On 24-Feb-2018 18:30, "'Prashant Panchal' via Materials & Welding" <materials-welding@googlegroups.com> wrote:
Please check gas backing is essential variable for welder qualification. 
On Sat, Feb 24, 2018 at 6:23 PM, sankar rao
If welder qualified with SS 
(GTAW Process),
He can weld CS ( GTAW Process)
Because of F.No's same for both SS &CS  for GTAW 
SS ---- F.NO 6.  SFA NO. 5.9
CS----- F.NO 6.   SFA NO. 5.18

On 24 Feb 2018 14:50, "'Prashant Panchal' via Materials & Welding" <materials-welding@ googlegroups.com> wrote:
Since he may have used backing gas for SS gtaw he will not be qualified for carbon steel as we do not use backing gas for cs material. 
Alternatively u will have to use backing gas for cs as well


On Sat, Feb 24, 2018 at 3:33 PM, PK M
Dear Sir,

If a welder is qualified with SS (Stainless Steel) GTAW,  He can weld CS Carbon steel GTAW? Need code Referance...

Thanks.
PKM

--
https://materials-welding. blogspot.com/
https://www.linkedin.com/ groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@ googlegroups.com.
Visit this group at https://groups.google.com/ group/materials-welding.
For more options, visit https://groups.google.com/d/ optout.

--
https://materials-welding. blogspot.com/
https://www.linkedin.com/ groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@ googlegroups.com.
Visit this group at https://groups.google.com/ group/materials-welding.
For more options, visit https://groups.google.com/d/ optout.

--
https://materials-welding. blogspot.com/
https://www.linkedin.com/ groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@ googlegroups.com.
Visit this group at https://groups.google.com/ group/materials-welding.
For more options, visit https://groups.google.com/d/ optout.

--
https://materials-welding. blogspot.com/
https://www.linkedin.com/ groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@ googlegroups.com.
Visit this group at https://groups.google.com/ group/materials-welding.
For more options, visit https://groups.google.com/d/ optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .