Skip to main content

RE: [MW:27363] Chromium limit to maintain back purging

API 582 Section 7.3 specified that "Back purging is required ……….. for a nominal chromium content greater than 2 ¼% ……."

 

 

Feng Lu, Ph.D., NDE Level III
Metallurgy and Welding Engineer

Zachry Industrial, Inc.
3600 West Sam Houston Pkwy South

Suite 200

Houston, TX 77042

luf@zachrygroup.com
Office: 713.979.2648
Cell: 512 797 5777
www.ZachryGroup.com

This e-mail may contain confidential and privileged material for the sole use of the intended recipient. Any review, use, distribution or disclosure by others is strictly prohibited. If you are not the intended recipient (or authorized to receive for the recipient), please contact the sender by reply e-mail and delete all copies of this message.

 

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of PGoswami
Sent: Wednesday, February 21, 2018 7:04 AM
To: materials-welding@googlegroups.com
Subject: RE: [MW:27362] Cromium limit to maintain back purging

 

This practice is considered to be a good engineering practices. BPV codes can't mandate all , many of such things has to come from the fabricators' sound engineering judgement and adopted practices.

 

Please see below the extract from API-RP-582, on the requirements of back purging.

 

P.Goswami.P.Eng, IWE.

Welding & Metallurgical Specialist

Linkedin: https://secure-web.cisco.com/1O4oLmpbUXp9Pyre9Qhqe1-sgFOkQg-b28jLfwQLaI9jtjE-SUzK8Du-3iwQ1tPgc3R7r_Rj7vc6X7YZ1rFbxwQfOuzvTKmGIqFBv8VLcexUdmtcyUO8SJKfVuj6mLUNZvt33r-_0q5jSc35ehC99Eqo62T_ZUL2GafUciEhmvMBfMZy4J6EYMsTYdxmelktc5UmGyTNvbBd-VsZ3Q6F2ZcqnLN7AAQUMyn2VRgpPUirKBx9Li9C_jHVRzrVaIGK8utzyHuKxVFfRJz6KU5pl7fKknjwxTtwP5jZHbqTvcVkUnpnLopInUQXDRAhVD4J7/https%3A%2F%2Fwww.linkedin.com%2Fin%2Fpradip-goswami-2999855%2F

Email:pgoswami@quickclic.net,pradip.goswami@gmail.com

M(in India-Till 26 Feb, 2018)- 8336816470

 

7.3 Back purging is required for the GTAW and GMAW processes for welding materials having a nominal chromium content greater than 2-1/4 %, unless the joint is ground or back gouged to sound metal.

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of pradip kumar Sil
Sent: February 21, 2018 3:09 PM
To: materials-welding <materials-welding@googlegroups.com>
Subject: Re: [MW:27361] Cromium limit to maintain back purging

 

Dear everybody,

Can anybody pls give me any code reference regarding this issue. I searched B31.1 , B31.3,  ASME but i did not find  minium chrimium percentage written on the code.

 

Is code silence regarding this issue.

 

Waiting for your valuable reply.

 

thanks in advance

 

regards

pradip

 

On 20 Feb 2018 12:19 pm, "Kannayeram Gnanapandithan" <kgpandithan@gmail.com> wrote:

ref B31.1 or B31.3, and lot of books 


THANKS & BEST REGARDS,

KG.PANDITHAN, BE, IWE,  AWS-CWI, CSWIP 3.1,

CONSULTANT-WELDING & QUALITY

Mobile no: +919940739349

 

On Tue, Feb 20, 2018 at 12:39 PM, pradip kumar Sil <pradipsil@gmail.com> wrote:

Dear Sir,

Can you pls provide me code references.

Thanks in advance

Pradip

 

On 20 Feb 2018 8:53 am, "Kannayeram Gnanapandithan" <kgpandithan@gmail.com> wrote:

Grater than 3% Cr, purging

 

On 20-Feb-2018 9:51 am, "pradip kumar Sil" <pradipsil@gmail.com> wrote:

Dear everybody,

Can anybody inform me minimum how much percentage of cromium limit to maintain back purging with code reference.

Thanks in advance

Pradip

--
https://secure-web.cisco.com/1WI-6rbflgL5uK9Y4-IUslNAhnocdtF8xz139qc_4NSxT4AFy48s2m1Hwiy-IpZY4kYNzgM2i8ZyxLZxkcPIONBBUQ_W-EOc7SYUlfQDVci3ue1h4hcjxlbWTVL7yeuql__X0eTq7xoS1AJnAlSrF9Jdg-STbPKMTTvuMGvVTps9gJQ3SLItKAACELeqp-ZIClE3WnGuz0oLWlTsgYgVqaUq4UFE9BWUI0iXUeYnknk5yFrXPiQmp19xkz6V1iZ_glkmGbekEZoAFxAHFggjAhD5FKS3YOPpPdmw3vCpMGtVpROZQUr2McS7lwHu3sJFN/https%3A%2F%2Fmaterials-welding.blogspot.com%2F
https://secure-web.cisco.com/1EmKVg9zmsSUuIKKNSSCleOqJianWGkf7P_NwVRTqdEkVSZz77pg54keAEr5xGMhOqGoRRA_QZN-QGKKnuuvgMNfzs6ZivbsLLxtsTfH6o8qY5Tm5KtkhguJd594j9OnKcBGCvgUOhxSG5iqceMTvoZYslP7d2awVW8S0QGGAk-s2mE980LoBy0LavhEfUntjWCs4cGQp1Ku9-RVvmmhWMTMIJ10bNA7ffn6XNSy3xOdZlSClJJmMwYJq-Owg-xqYHpfoxToxDRQyty-xs-Apj1KFhF-aJ5eHzEk_6Cb2g4NVFt0jFnRbE0LTBqc4R8rb/https%3A%2F%2Fwww.linkedin.com%2Fgroups%2F122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://secure-web.cisco.com/1PNtnl104TjT9pZ09CLGiWV5tytAIpfDaOM2jRVEpYM-WpgLinZlSdkAehsRrYrHGhIstPIqbLkxbJpxLbnNSdw--W7wKUOLg88YHDMhec7Mv2Di3RERDepqD-teSEDST7qJM-m7y_PYeiM8-3dDsFHMNPlglzmOwYy8k85UAeqwy2rFgZ3Hb3j2cfXZwGZvLOCfPqlZ2RapfgnwDnhpX6X_ckAcmi1fgmDQIB1Lj8sMIu7AWzpKRfIEbnloYSEdYfEH41_AxDWn_Cd-0hYmfakdElIcRYyqgD9KC54ZQNaRGP5S6wjDB7HTB8lf4dyyCXWjardswJvKYu4l7cJY9Mw/https%3A%2F%2Fgroups.google.com%2Fgroup%2Fmaterials-welding.
For more options, visit https://secure-web.cisco.com/1_iL-1MHNDLbMAnFXdt80pnrQsr0VKpaUcfiw-EnxayfVtbrOlhUSMhpsMiy8XXh8vzYSFFJeS87-JvMRybpOJ3HL5cE6JCyzbR7JV4H5QlK1_cLfJwwFSgfU_fLOwP3U0z3TI6YUcYOdjHRikR_JZrEz3bGe9BoC790Y3-pZqKLdsMsW1E-OAd8PIGIfEEyHqAuILGsuHAnFSEGz0DqDQzUxf_9r_XQHq6bWVytsALoKlAOaoWsQLVSRsPHrNgHA_V_1l4bhmwz55DZnj-k-gVlcdvZxcNaNlItVYfGPK58RCwiZMIhMEseaHvnSfBPp0KRGYaLEdQV3n4ab4GEYVg/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

--
https://secure-web.cisco.com/1WI-6rbflgL5uK9Y4-IUslNAhnocdtF8xz139qc_4NSxT4AFy48s2m1Hwiy-IpZY4kYNzgM2i8ZyxLZxkcPIONBBUQ_W-EOc7SYUlfQDVci3ue1h4hcjxlbWTVL7yeuql__X0eTq7xoS1AJnAlSrF9Jdg-STbPKMTTvuMGvVTps9gJQ3SLItKAACELeqp-ZIClE3WnGuz0oLWlTsgYgVqaUq4UFE9BWUI0iXUeYnknk5yFrXPiQmp19xkz6V1iZ_glkmGbekEZoAFxAHFggjAhD5FKS3YOPpPdmw3vCpMGtVpROZQUr2McS7lwHu3sJFN/https%3A%2F%2Fmaterials-welding.blogspot.com%2F
https://secure-web.cisco.com/1EmKVg9zmsSUuIKKNSSCleOqJianWGkf7P_NwVRTqdEkVSZz77pg54keAEr5xGMhOqGoRRA_QZN-QGKKnuuvgMNfzs6ZivbsLLxtsTfH6o8qY5Tm5KtkhguJd594j9OnKcBGCvgUOhxSG5iqceMTvoZYslP7d2awVW8S0QGGAk-s2mE980LoBy0LavhEfUntjWCs4cGQp1Ku9-RVvmmhWMTMIJ10bNA7ffn6XNSy3xOdZlSClJJmMwYJq-Owg-xqYHpfoxToxDRQyty-xs-Apj1KFhF-aJ5eHzEk_6Cb2g4NVFt0jFnRbE0LTBqc4R8rb/https%3A%2F%2Fwww.linkedin.com%2Fgroups%2F122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://secure-web.cisco.com/1PNtnl104TjT9pZ09CLGiWV5tytAIpfDaOM2jRVEpYM-WpgLinZlSdkAehsRrYrHGhIstPIqbLkxbJpxLbnNSdw--W7wKUOLg88YHDMhec7Mv2Di3RERDepqD-teSEDST7qJM-m7y_PYeiM8-3dDsFHMNPlglzmOwYy8k85UAeqwy2rFgZ3Hb3j2cfXZwGZvLOCfPqlZ2RapfgnwDnhpX6X_ckAcmi1fgmDQIB1Lj8sMIu7AWzpKRfIEbnloYSEdYfEH41_AxDWn_Cd-0hYmfakdElIcRYyqgD9KC54ZQNaRGP5S6wjDB7HTB8lf4dyyCXWjardswJvKYu4l7cJY9Mw/https%3A%2F%2Fgroups.google.com%2Fgroup%2Fmaterials-welding.
For more options, visit https://secure-web.cisco.com/1_iL-1MHNDLbMAnFXdt80pnrQsr0VKpaUcfiw-EnxayfVtbrOlhUSMhpsMiy8XXh8vzYSFFJeS87-JvMRybpOJ3HL5cE6JCyzbR7JV4H5QlK1_cLfJwwFSgfU_fLOwP3U0z3TI6YUcYOdjHRikR_JZrEz3bGe9BoC790Y3-pZqKLdsMsW1E-OAd8PIGIfEEyHqAuILGsuHAnFSEGz0DqDQzUxf_9r_XQHq6bWVytsALoKlAOaoWsQLVSRsPHrNgHA_V_1l4bhmwz55DZnj-k-gVlcdvZxcNaNlItVYfGPK58RCwiZMIhMEseaHvnSfBPp0KRGYaLEdQV3n4ab4GEYVg/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

--
https://secure-web.cisco.com/1WI-6rbflgL5uK9Y4-IUslNAhnocdtF8xz139qc_4NSxT4AFy48s2m1Hwiy-IpZY4kYNzgM2i8ZyxLZxkcPIONBBUQ_W-EOc7SYUlfQDVci3ue1h4hcjxlbWTVL7yeuql__X0eTq7xoS1AJnAlSrF9Jdg-STbPKMTTvuMGvVTps9gJQ3SLItKAACELeqp-ZIClE3WnGuz0oLWlTsgYgVqaUq4UFE9BWUI0iXUeYnknk5yFrXPiQmp19xkz6V1iZ_glkmGbekEZoAFxAHFggjAhD5FKS3YOPpPdmw3vCpMGtVpROZQUr2McS7lwHu3sJFN/https%3A%2F%2Fmaterials-welding.blogspot.com%2F
https://secure-web.cisco.com/1EmKVg9zmsSUuIKKNSSCleOqJianWGkf7P_NwVRTqdEkVSZz77pg54keAEr5xGMhOqGoRRA_QZN-QGKKnuuvgMNfzs6ZivbsLLxtsTfH6o8qY5Tm5KtkhguJd594j9OnKcBGCvgUOhxSG5iqceMTvoZYslP7d2awVW8S0QGGAk-s2mE980LoBy0LavhEfUntjWCs4cGQp1Ku9-RVvmmhWMTMIJ10bNA7ffn6XNSy3xOdZlSClJJmMwYJq-Owg-xqYHpfoxToxDRQyty-xs-Apj1KFhF-aJ5eHzEk_6Cb2g4NVFt0jFnRbE0LTBqc4R8rb/https%3A%2F%2Fwww.linkedin.com%2Fgroups%2F122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://secure-web.cisco.com/1PNtnl104TjT9pZ09CLGiWV5tytAIpfDaOM2jRVEpYM-WpgLinZlSdkAehsRrYrHGhIstPIqbLkxbJpxLbnNSdw--W7wKUOLg88YHDMhec7Mv2Di3RERDepqD-teSEDST7qJM-m7y_PYeiM8-3dDsFHMNPlglzmOwYy8k85UAeqwy2rFgZ3Hb3j2cfXZwGZvLOCfPqlZ2RapfgnwDnhpX6X_ckAcmi1fgmDQIB1Lj8sMIu7AWzpKRfIEbnloYSEdYfEH41_AxDWn_Cd-0hYmfakdElIcRYyqgD9KC54ZQNaRGP5S6wjDB7HTB8lf4dyyCXWjardswJvKYu4l7cJY9Mw/https%3A%2F%2Fgroups.google.com%2Fgroup%2Fmaterials-welding.
For more options, visit https://secure-web.cisco.com/1_iL-1MHNDLbMAnFXdt80pnrQsr0VKpaUcfiw-EnxayfVtbrOlhUSMhpsMiy8XXh8vzYSFFJeS87-JvMRybpOJ3HL5cE6JCyzbR7JV4H5QlK1_cLfJwwFSgfU_fLOwP3U0z3TI6YUcYOdjHRikR_JZrEz3bGe9BoC790Y3-pZqKLdsMsW1E-OAd8PIGIfEEyHqAuILGsuHAnFSEGz0DqDQzUxf_9r_XQHq6bWVytsALoKlAOaoWsQLVSRsPHrNgHA_V_1l4bhmwz55DZnj-k-gVlcdvZxcNaNlItVYfGPK58RCwiZMIhMEseaHvnSfBPp0KRGYaLEdQV3n4ab4GEYVg/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

 

--
https://secure-web.cisco.com/1WI-6rbflgL5uK9Y4-IUslNAhnocdtF8xz139qc_4NSxT4AFy48s2m1Hwiy-IpZY4kYNzgM2i8ZyxLZxkcPIONBBUQ_W-EOc7SYUlfQDVci3ue1h4hcjxlbWTVL7yeuql__X0eTq7xoS1AJnAlSrF9Jdg-STbPKMTTvuMGvVTps9gJQ3SLItKAACELeqp-ZIClE3WnGuz0oLWlTsgYgVqaUq4UFE9BWUI0iXUeYnknk5yFrXPiQmp19xkz6V1iZ_glkmGbekEZoAFxAHFggjAhD5FKS3YOPpPdmw3vCpMGtVpROZQUr2McS7lwHu3sJFN/https%3A%2F%2Fmaterials-welding.blogspot.com%2F
https://secure-web.cisco.com/1EmKVg9zmsSUuIKKNSSCleOqJianWGkf7P_NwVRTqdEkVSZz77pg54keAEr5xGMhOqGoRRA_QZN-QGKKnuuvgMNfzs6ZivbsLLxtsTfH6o8qY5Tm5KtkhguJd594j9OnKcBGCvgUOhxSG5iqceMTvoZYslP7d2awVW8S0QGGAk-s2mE980LoBy0LavhEfUntjWCs4cGQp1Ku9-RVvmmhWMTMIJ10bNA7ffn6XNSy3xOdZlSClJJmMwYJq-Owg-xqYHpfoxToxDRQyty-xs-Apj1KFhF-aJ5eHzEk_6Cb2g4NVFt0jFnRbE0LTBqc4R8rb/https%3A%2F%2Fwww.linkedin.com%2Fgroups%2F122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://secure-web.cisco.com/1PNtnl104TjT9pZ09CLGiWV5tytAIpfDaOM2jRVEpYM-WpgLinZlSdkAehsRrYrHGhIstPIqbLkxbJpxLbnNSdw--W7wKUOLg88YHDMhec7Mv2Di3RERDepqD-teSEDST7qJM-m7y_PYeiM8-3dDsFHMNPlglzmOwYy8k85UAeqwy2rFgZ3Hb3j2cfXZwGZvLOCfPqlZ2RapfgnwDnhpX6X_ckAcmi1fgmDQIB1Lj8sMIu7AWzpKRfIEbnloYSEdYfEH41_AxDWn_Cd-0hYmfakdElIcRYyqgD9KC54ZQNaRGP5S6wjDB7HTB8lf4dyyCXWjardswJvKYu4l7cJY9Mw/https%3A%2F%2Fgroups.google.com%2Fgroup%2Fmaterials-welding.
For more options, visit https://secure-web.cisco.com/1_iL-1MHNDLbMAnFXdt80pnrQsr0VKpaUcfiw-EnxayfVtbrOlhUSMhpsMiy8XXh8vzYSFFJeS87-JvMRybpOJ3HL5cE6JCyzbR7JV4H5QlK1_cLfJwwFSgfU_fLOwP3U0z3TI6YUcYOdjHRikR_JZrEz3bGe9BoC790Y3-pZqKLdsMsW1E-OAd8PIGIfEEyHqAuILGsuHAnFSEGz0DqDQzUxf_9r_XQHq6bWVytsALoKlAOaoWsQLVSRsPHrNgHA_V_1l4bhmwz55DZnj-k-gVlcdvZxcNaNlItVYfGPK58RCwiZMIhMEseaHvnSfBPp0KRGYaLEdQV3n4ab4GEYVg/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

--
https://secure-web.cisco.com/1WI-6rbflgL5uK9Y4-IUslNAhnocdtF8xz139qc_4NSxT4AFy48s2m1Hwiy-IpZY4kYNzgM2i8ZyxLZxkcPIONBBUQ_W-EOc7SYUlfQDVci3ue1h4hcjxlbWTVL7yeuql__X0eTq7xoS1AJnAlSrF9Jdg-STbPKMTTvuMGvVTps9gJQ3SLItKAACELeqp-ZIClE3WnGuz0oLWlTsgYgVqaUq4UFE9BWUI0iXUeYnknk5yFrXPiQmp19xkz6V1iZ_glkmGbekEZoAFxAHFggjAhD5FKS3YOPpPdmw3vCpMGtVpROZQUr2McS7lwHu3sJFN/https%3A%2F%2Fmaterials-welding.blogspot.com%2F
https://secure-web.cisco.com/1EmKVg9zmsSUuIKKNSSCleOqJianWGkf7P_NwVRTqdEkVSZz77pg54keAEr5xGMhOqGoRRA_QZN-QGKKnuuvgMNfzs6ZivbsLLxtsTfH6o8qY5Tm5KtkhguJd594j9OnKcBGCvgUOhxSG5iqceMTvoZYslP7d2awVW8S0QGGAk-s2mE980LoBy0LavhEfUntjWCs4cGQp1Ku9-RVvmmhWMTMIJ10bNA7ffn6XNSy3xOdZlSClJJmMwYJq-Owg-xqYHpfoxToxDRQyty-xs-Apj1KFhF-aJ5eHzEk_6Cb2g4NVFt0jFnRbE0LTBqc4R8rb/https%3A%2F%2Fwww.linkedin.com%2Fgroups%2F122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://secure-web.cisco.com/1PNtnl104TjT9pZ09CLGiWV5tytAIpfDaOM2jRVEpYM-WpgLinZlSdkAehsRrYrHGhIstPIqbLkxbJpxLbnNSdw--W7wKUOLg88YHDMhec7Mv2Di3RERDepqD-teSEDST7qJM-m7y_PYeiM8-3dDsFHMNPlglzmOwYy8k85UAeqwy2rFgZ3Hb3j2cfXZwGZvLOCfPqlZ2RapfgnwDnhpX6X_ckAcmi1fgmDQIB1Lj8sMIu7AWzpKRfIEbnloYSEdYfEH41_AxDWn_Cd-0hYmfakdElIcRYyqgD9KC54ZQNaRGP5S6wjDB7HTB8lf4dyyCXWjardswJvKYu4l7cJY9Mw/https%3A%2F%2Fgroups.google.com%2Fgroup%2Fmaterials-welding.
For more options, visit https://secure-web.cisco.com/1_iL-1MHNDLbMAnFXdt80pnrQsr0VKpaUcfiw-EnxayfVtbrOlhUSMhpsMiy8XXh8vzYSFFJeS87-JvMRybpOJ3HL5cE6JCyzbR7JV4H5QlK1_cLfJwwFSgfU_fLOwP3U0z3TI6YUcYOdjHRikR_JZrEz3bGe9BoC790Y3-pZqKLdsMsW1E-OAd8PIGIfEEyHqAuILGsuHAnFSEGz0DqDQzUxf_9r_XQHq6bWVytsALoKlAOaoWsQLVSRsPHrNgHA_V_1l4bhmwz55DZnj-k-gVlcdvZxcNaNlItVYfGPK58RCwiZMIhMEseaHvnSfBPp0KRGYaLEdQV3n4ab4GEYVg/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

--
https://secure-web.cisco.com/1WI-6rbflgL5uK9Y4-IUslNAhnocdtF8xz139qc_4NSxT4AFy48s2m1Hwiy-IpZY4kYNzgM2i8ZyxLZxkcPIONBBUQ_W-EOc7SYUlfQDVci3ue1h4hcjxlbWTVL7yeuql__X0eTq7xoS1AJnAlSrF9Jdg-STbPKMTTvuMGvVTps9gJQ3SLItKAACELeqp-ZIClE3WnGuz0oLWlTsgYgVqaUq4UFE9BWUI0iXUeYnknk5yFrXPiQmp19xkz6V1iZ_glkmGbekEZoAFxAHFggjAhD5FKS3YOPpPdmw3vCpMGtVpROZQUr2McS7lwHu3sJFN/https%3A%2F%2Fmaterials-welding.blogspot.com%2F
https://secure-web.cisco.com/1EmKVg9zmsSUuIKKNSSCleOqJianWGkf7P_NwVRTqdEkVSZz77pg54keAEr5xGMhOqGoRRA_QZN-QGKKnuuvgMNfzs6ZivbsLLxtsTfH6o8qY5Tm5KtkhguJd594j9OnKcBGCvgUOhxSG5iqceMTvoZYslP7d2awVW8S0QGGAk-s2mE980LoBy0LavhEfUntjWCs4cGQp1Ku9-RVvmmhWMTMIJ10bNA7ffn6XNSy3xOdZlSClJJmMwYJq-Owg-xqYHpfoxToxDRQyty-xs-Apj1KFhF-aJ5eHzEk_6Cb2g4NVFt0jFnRbE0LTBqc4R8rb/https%3A%2F%2Fwww.linkedin.com%2Fgroups%2F122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://secure-web.cisco.com/1PNtnl104TjT9pZ09CLGiWV5tytAIpfDaOM2jRVEpYM-WpgLinZlSdkAehsRrYrHGhIstPIqbLkxbJpxLbnNSdw--W7wKUOLg88YHDMhec7Mv2Di3RERDepqD-teSEDST7qJM-m7y_PYeiM8-3dDsFHMNPlglzmOwYy8k85UAeqwy2rFgZ3Hb3j2cfXZwGZvLOCfPqlZ2RapfgnwDnhpX6X_ckAcmi1fgmDQIB1Lj8sMIu7AWzpKRfIEbnloYSEdYfEH41_AxDWn_Cd-0hYmfakdElIcRYyqgD9KC54ZQNaRGP5S6wjDB7HTB8lf4dyyCXWjardswJvKYu4l7cJY9Mw/https%3A%2F%2Fgroups.google.com%2Fgroup%2Fmaterials-welding.
For more options, visit https://secure-web.cisco.com/1_iL-1MHNDLbMAnFXdt80pnrQsr0VKpaUcfiw-EnxayfVtbrOlhUSMhpsMiy8XXh8vzYSFFJeS87-JvMRybpOJ3HL5cE6JCyzbR7JV4H5QlK1_cLfJwwFSgfU_fLOwP3U0z3TI6YUcYOdjHRikR_JZrEz3bGe9BoC790Y3-pZqKLdsMsW1E-OAd8PIGIfEEyHqAuILGsuHAnFSEGz0DqDQzUxf_9r_XQHq6bWVytsALoKlAOaoWsQLVSRsPHrNgHA_V_1l4bhmwz55DZnj-k-gVlcdvZxcNaNlItVYfGPK58RCwiZMIhMEseaHvnSfBPp0KRGYaLEdQV3n4ab4GEYVg/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...