Re: [MW:21732] Notch Toughness Properties of WPQR.

Dear Gandhi
1st thing why you did normalizing for so much time?
If you check the all plates manufactures mtc they did normalizing generally I range of 1.25 to 1.5 min per mm of plates thickness . I think this high time heat treatment hamper the values.
2nd thing as per my knowledge you cannot subsize the samples sizes if you are able to get standerd size of 10 by 10 as per UG 84 or at least 8 by 8 mm.
can you tell us the justification?
3rd thing E 7018 is not suitable for normalized condition we used generally electrodes of E 8018 series and get good results in my ladt company due to higher tensile valus of electrods.
Waiting of responses from welding specialists.

Intekhab Alam Ansari
Lead Engineer QA/QC
RIL J3 Expansion Project
MTF/RTF Area

On 27 Aug 2014 17:52, "C.Muni" <cmkfc07@gmail.com> wrote:
This grade is not suitable for the test temperature you indicated.Please check again.

Regards,


 Muniiandii.Ci MBA,
NDT Level II,
ISO 9001,14001 Lead Auditor,


Mobile:99947 65591

Growth is the only evidence of life.


On Tue, Aug 19, 2014 at 1:42 PM, 'CHINTUKUMAR GANDHI' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Dear Experts,

Greetings of the day.

I came to an issue in WPQR of P No. 1 Group 2 Base metal in CVN Impact testing of weld and haz. Design Code is ASME Sec. VIII Div. 1 Ed. 2013 & ASME Sec. IX Ed. 2013.

Base Metal Thk. 25 mm. SA 516 Gr. 70
PWHT: Normalizing at 920+/-10º C.
Holding Period 65 Minutes.
Welding Process SMAW (Manual)
Electrode Used: 3.15 & 4.0 mm. E7018-1 (Impact tested in as welded condition).
Position: 3 G Uphill (Stringer/ Weave Bead)

CVN Impact test results of HAZ: 
Test Temp. -57º C (Temp. reduction applicable)
Specimen size: 10 x 5 x 55 mm.
Values in Joules HAZ Top Side- 5, 19.5, 4 (Average 9.50)
Values in Joules HAZ Bottom Side- 4.5, 4, 17.5 (Average 8.67)
Values reqd. for sub size specimen: Individual min. 8 J & Min. Average 10 J.

CVN Impact test results of Weld:
Test Temp. -46º C (Temp. reduction applicable)
Specimen size: 10 x 10 x 55 mm.
Values in Joules - 9, 14.5, 8.5 (Average 10.67)
Values reqd. for Std. size specimen: Individual min. 16 J & Min. Average 20 J.

What shall be the reason of failure? Is electrode selection OK?

Awaiting for your prompt favorable response at the earliest.

Thanks & regards,


C. R. GANDHI

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...