Wednesday, August 27, 2014

Re: [MW:21723] Notch Toughness Properties of WPQR.

Dear,

I think E7018-1 will not give properties at temp. you mentioned.
Best Regards,
Mohit Aggarwal.

Dear Experts,

Greetings of the day.

I came to an issue in WPQR of P No. 1 Group 2 Base metal in CVN Impact testing of weld and haz. Design Code is ASME Sec. VIII Div. 1 Ed. 2013 & ASME Sec. IX Ed. 2013.

Base Metal Thk. 25 mm. SA 516 Gr. 70
PWHT: Normalizing at 920+/-10º C.
Holding Period 65 Minutes.
Welding Process SMAW (Manual)
Electrode Used: 3.15 & 4.0 mm. E7018-1 (Impact tested in as welded condition).
Position: 3 G Uphill (Stringer/ Weave Bead)

CVN Impact test results of HAZ: 
Test Temp. -57º C (Temp. reduction applicable)
Specimen size: 10 x 5 x 55 mm.
Values in Joules HAZ Top Side- 5, 19.5, 4 (Average 9.50)
Values in Joules HAZ Bottom Side- 4.5, 4, 17.5 (Average 8.67)
Values reqd. for sub size specimen: Individual min. 8 J & Min. Average 10 J.

CVN Impact test results of Weld:
Test Temp. -46º C (Temp. reduction applicable)
Specimen size: 10 x 10 x 55 mm.
Values in Joules - 9, 14.5, 8.5 (Average 10.67)
Values reqd. for Std. size specimen: Individual min. 16 J & Min. Average 20 J.

What shall be the reason of failure? Is electrode selection OK?

Awaiting for your prompt favorable response at the earliest.

Thanks & regards,


C. R. GANDHI

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...