Skip to main content

Re: [MW:21456] welding ss pipes with R316LT1

You can try Vapor blasting if approachable.

S.N.Bagchi


On Thursday, July 24, 2014 10:57 AM, Abi Joseph <joseph@dnhsecheron.net> wrote:


Dear Friend

I really don't think this is a forum to promote a particular manufacturer's product & services, but to share the technical knowledge, experience and expertise, of each of the valued forum members. 
 
Fond Regards,
Abi Joseph

Dear Mr Prem Nautiyal - Your view pl.



From: "Amitabha.Bhattacharya@voestalpine.com" <Amitabha.Bhattacharya@voestalpine.com>
To: materials-welding@googlegroups.com
Sent: Monday, July 21, 2014 3:28 PM
Subject: RE: [MW:21436] welding ss pipes with R316LT1

Hi Deepak,
 
There is no way you can avoid slag going to otherside-in fact purpose of a flux-cored TIG filler  is to produce fluid slag acting deemed purging.
 
I would suggest you may look at the attached PDS of Avesta 316L/SKR -4D electrodes recommended for such applications.
Hope this helps..
Thanks
 
With Regards
Amitabha Bhattacharya
Head - Application Technology
 
voestalpine Bohler Welding India Pvt. Ltd.
voestalpine Bohler Application Technology Centre
A-140, Metropolitan, ground floor
Road no. 23, Wagle Industrial Estate
Thane – 400604, India
T. +91-22-2582 8855
F. +91-22-2857 4445
M. +91-98 33998246
amitabha.bhattacharya@voestalpine.com
www.voestalpine.com/welding
voestalpine – One step ahead
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of DEEPAK cb
Sent: Monday, July 21, 2014 2:18 PM
To: materials-welding@googlegroups.com
Subject: [MW:21434] welding ss pipes with R316LT1
 
Dear All
 
I need to do some repair works in 316L pipes. So purging in these pipes are a problem and so am planning to use R316LT1-5 from the manufacture kobelco. Welding process is TIG. As per the manufacture R316LT1 does not requires any purging and can do the root run using the filler wire. But slag will be formed in the back side of the root. IS there any way to remove these  slags as it is drinking water line.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...