Tuesday, May 20, 2014

RE: [MW:20855] SS material is Corroded

Be careful when using buffing or wheel which may spread out iron or rust  and cause rust again.

Previously , we had used a chemical to remove iron out from stainless steel surface.

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Shomenath Bagchi
Sent: Monday, May 19, 2014 9:39 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:20854] SS material is Corroded

 

Surface cleaning and passivization with nitric aid will improve the situation.

S.N.Bagchi

On Monday, May 19, 2014 4:15 AM, as_sundarrajan via Materials & Welding <materials-welding@googlegroups.com> wrote:

 


Pickling and passivation will help you the larger extent

Sent from C7 mobile

-----Original Message-----
From: Sri Ram
Sent:  18/05/2014, 1:38  PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:20841] SS material is Corroded


Hi brother,

you can remove the corrosion by ss buffing wheel.check after 1week , still
the same corrision occurs means , you cut 25mm either side of  the pipe and
remove the weld joint metal.

do fitup and reweld .







On Sun, May 18, 2014 at 8:01 AM, zubair <zubair.me@gmail.com> wrote:

>
>
> Dear All,
>
>
> By Mistake our fabricator use ms buffing wheel instead of SS buffing wheel
> . what happen after some time SS material surface corrosion appears.
>
>
> Please tell us remedy how to remove corrosion .
>
>
> thanx
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
>
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups
> "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an
> email to materials-welding+unsubscribe@googlegroups.com.
> For more options, visit https://groups.google.com/d/optout.
>



--
Regards/Thanks

S.Sriram
L & T
Saudi Arabia
Mobile No. 00966545221548

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...