[MW:20892] Re: Major requirement between LAS and CS vessels

I believe LAS stands for Low Alloy Steel
Some of the major requirements are dictated as follows
- For Carbon Steel, PWHT requirements are always above 19mm thickness, whereas LAS being Cr-Mo steel in general are Hardenable, so pre-heat and PWHT can be requirements irrespective of material thickness like P-91 and P-22
- For Carbon Steel, Electrode Qualification test is not mandatory and we can select on the basic of its Material Test Certificate, whereas for Low Alloy Steel, Electrode Qualification Test is mandatory which include Chemical Pad test also for each batch (PS: In Carbon Steel, however LTCS requires Electrode Qualification test)
- For Carbon Steel, no requirement of PMI (Positive Material Identification) whereas for LAS , PMI is mandatory

Regards
Arunabh 
Engineers India Limited

On Friday, May 16, 2014 4:34:48 PM UTC+5:30, ganesh mariappan wrote:
can anybody clarify my doubt that, what is major requirement between asme CS and LAS vessels?

Best regards,
Ganesh.M

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...