Attached is a copy of 2013 ScIX QW-202.1.  The following is my interpretation of the requirements.

 

Three conditions are set up in the case of a specimen failure:

 

1)     (2nd paragraph) Failure was caused by something unrelated to the welding conditions.  This could be a failure of the grips, a nick in the specimen, an error in machining, power failure during the test, etc.  In this case one for one replacement of the specimen from the original PQR coupon or a new test coupon welded with the same parameters/conditions may be made and the additional specimen tested.

 

2)    (4th paragraph) If the failure was caused by a problem that requires a change in essential or supplementary essential variables to correct the problem, then a new PQR test plate must be welded and all tests repeated.  Personally, I don’t see how the original PQR test(s) would be valid if the essential (or supplementary essential) variables have changed. 

 

3)    (5th paragraph) If the failure was caused by a problem related to welding but that requires a change not affecting the original essential or supplementary essential variables, then a new coupon can be welded and the failed test repeated.  The changes made to the non-essential variables or other parameters to obtain the acceptable test(s) must be addressed on the WPS.  In this case it is one for one replacement. 

 

Typically a failure of a PQR test will be the result of condition 2) above.  In my experience, use of condition 3) is rare. 

 

Just my opinion along with a strong belief that a short cut isn’t necessarily the quickest route to anywhere.  Good luck.

 

John A. Henning

Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of george.dilintas@gr.bureauveritas.com
Sent: Wednesday, April 30, 2014 9:50 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:20712] ASME SEC IX QW202.1

 

Sorry dear Meisam
I am not getting your point

best regards

Dr. Georgios Dilintas

Authorized Nuclear Inspector
Authorized Inspector Supervisor
API 510 Inspector

I&F REGIONAL TECHNICAL MANAGER
BUREAU VERITAS HELLAS

Tel: +30 210 40 63 113/4
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04
(See attached file: Dilintas_George.vcf)


meisam shokri arfaei ---30/04/2014 15:19:24---Dear Dilinates, There is no problem if something added or deleted to the main topic in the

From: meisam shokri arfaei <meisamshokri@gmail.com>
To: materials-welding@googlegroups.com
Date: 30/04/2014 15:19
Subject: Re: [MW:20708] ASME SEC IX QW202.1
Sent by: materials-welding@googlegroups.com





Dear Dilinates,
There is no problem if something added or deleted to the main topic in the next para. in any standard or technical documents and with some new conditions. Those are exactly exceptions.

Regards


On Wed, Apr 30, 2014 at 12:34 PM, <george.dilintas@gr.bureauveritas.com> wrote:


I disagree
Please read carefully: It is written in the 1st paragraph of QW 202.1 "If any test specimen required by QW-451 fails to meet the applicable acceptance criteria, the test coupon shall be considered as failed"


best regards

Dr. Georgios Dilintas

Authorized Nuclear Inspector
Authorized Inspector Supervisor
API 510 Inspector

I&F REGIONAL TECHNICAL MANAGER
BUREAU VERITAS HELLAS

Tel: +30 210 40 63 113/4
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04

(See attached file: Dilintas_George.vcf)


meisam shokri arfaei ---29/04/2014 15:53:13---Dear Tulasi, 1 new specimen for 1 failed specimen (but just from the same test coupon).

From:
meisam shokri arfaei <meisamshokri@gmail.com>
To:
materials-welding@googlegroups.com
Date:
29/04/2014 15:53
Subject:
Re: [MW:20695] ASME SEC IX QW202.1
Sent by:
materials-welding@googlegroups.com






Dear Tulasi,

1 new specimen for 1 failed specimen (but just from the same test coupon).

Regards 


On Tue, Apr 29, 2014 at 10:36 AM, SWI <tulasiramus@gmail.com> wrote:

Thanks for the info,

Please note that QW202.1 also allows for retesting ( after considering all ifs & buts in the code/ QW153) from the same test coupon. Now my question is, if one tensile specimen fails, how many additional test specimens shall be tested.

 

On Monday, April 28, 2014 2:41:28 PM UTC+3, sina wrote:
Dear friend,

If any specimen fails to meet the requirements, the test coupon consider to be failed and a new test coupon shall prepare. (It could be with the same parameters or changed parameters)

Regards


On Mon, Apr 28, 2014 at 10:46 AM, STR <tulas...@gmail.com> wrote:

Friends,

Good Morning,

With reference to ASME Sec IX:

1. If one tensile specimen failed the requirement of QW153
2. How many additional specimens are to be tested QW202.1


Regards,
Tulasi Ram

--
To post to this group, send email to
material...@googlegroups.com
To unsubscribe from this group, send email to
materials-weld...@googlegroups.com

For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-weld...@googlegroups.com.

For more options, visit
https://groups.google.com/d/optout.





--
M. Shokri Arfaei
ISA-ISTS - Metallurgy Lab. Manager
ASNT NDT Level III
International Welding Engineer


Tel.: +98 21 66282127
Fax: +98 21 66282779
Mob.:+98 912 1394023


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.





--
M. Shokri Arfaei
ISA-ISTS - Metallurgy Lab. Manager
ASNT NDT Level III
International Welding Engineer


Tel.: +98 21 66282127
Fax: +98 21 66282779
Mob.:+98 912 1394023


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.




--
M. Shokri Arfaei

ISA-ISTS - Metallurgy Lab. Manager
ASNT NDT Level III
International Welding Engineer

Tel.: +98 21 66282127
Fax: +98 21 66282779
Mob.:+98 912 1394023


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...