Sir,

Thanks for your response. Can you give any reference for “if it delay not advisable to tack weld and keep for longtime. 2.5minutes/mm holding time ”

 

S.Binoy

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of kannayeram gnanapandithan
Sent: Monday, April 29, 2013 10:59 AM
To: materials-welding
Subject: Re: [MW:17585] Pre heat requirements for tack welding in P91

 

1.yes,but it is not good practice to tack weld on the job. if u take full welding immediately after tack weld it is ok, if it delay not advisable to tack weld and keep for longtime. 2.5minutes/mm holding time 

Pandithan

Welding Consultant

 

On Mon, Apr 29, 2013 at 11:56 AM, Lalu r p <lalucpt@gmail.com> wrote:

Dear Binoy 

 

When I was working in a power project in India as per Client's Requirement for P91 joints we used to keep the joints on external clamps and weld directly after the proper preheating and purging.for tubes as well as pipes we followed the same method.Direct tack welding was not allowed by the client.Correct me if i am wrong.

 

Thanks &Regards

LALU R.P

 

On Sun, Apr 28, 2013 at 10:39 AM, Binoy Soman <binoy.spp@daelim.co.kr> wrote:

Dear Experts,

 

Regarding the subject mentioned, kindly clarify my following doubts.

(a)    Preheating required for P91 as per B 31.1 is 200°C (mini). Does it mean that this Pre heat shall be given for tacking also.

(b)   PWHT holding time for P91 mentioned in B 31.1 is 1 hr/25 mm; minimum 30 minutes. Does it mean that if the thickness is 6/10/12.5 mm the holding time is 30 minutes & for 15 ,20,30,40 mm the holding time is 36  48,72,96 minutes respectively.

(c)    I got some special heating curves for P 91 from our group. But Kindly explain about the reference /standard used for preparation of this heat curve ( eg- why the preheat maintenance is 4 hours & again free cooling).

 

S.Binoy

 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...