Dear Azam,
 
I missed your email in the first place. Strictly as per Clause 5.2 of SA 333-2010 specification addition of these alloying elements are not permitted. However some of the alloying elements may come from the scrap used for steel melting.
 
What's the quantity involved? and what're the design requirements ?
 
A re-check of  chemistry by OES spectroscopy would be advisable. If the results of OES conforms to the  results of manufacture's "MTR",  then material is  to be discarded.
 
If the OES results do not pick up any of the alloying elements as  indicated below, then it would be  projects' discretion (i.e Client. EPC contractor and fabricator joint acceptance).
 
However talk to the mill in parallel and see if replacement is available , without jeopardizing manufacturing schedule.
 

Pradip Goswami,P.Eng.IWE

Welding & Metallurgical Specialist

Ontario, Canada.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

5.2 When  Grades 1, 6, or 10 are ordered under this specification (SA 333), supplying an alloy grade that specifically requires the addition of any element other than those listed for the ordered grade in Table 1 is not permitted. However, the addition of elements required for the deoxidation of the steel is permitted



From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of george.dilintas@gr.bureauveritas.com
Sent: Saturday, March 30, 2013 9:05 AM
To: materials-welding
Subject: Re: [MW:17256] Re: ASME SA 333 Gr. 6 Chemical composition

Sorry
But which of the additional elements is used for deoxidazation?
Usually for deoxidazation Al or Ca is used
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager


  From: sajeed zaheer [sajeed7674@gmail.com]
  Sent: 03/30/2013 11:08 AM ZE4
  To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
  Subject: Re: [MW:17254] Re: ASME SA 333 Gr. 6 Chemical composition


Dear Azam,
as per sec 8 div 1 partA  pg.550 para 5 chemical composition,

THE ADDITION OF ELEMENT REQUIRED FOR THE DEOXIDATION OF THE STEEL IS PERMITTED. AND YOU CAN ACCEPT THE ABOVE MENTION MTC AS PER THIS PARAGRAPH. 


On Wed, Mar 27, 2013 at 1:53 PM, Azam Mohd <azam1976@gmail.com> wrote:

Dear All Experts,

Please provide your feedback for below query with some technical justification or code reference.

 

Thanks & Regards,

Mohd. Azam


On Tue, Mar 19, 2013 at 5:09 PM, Azam Mohd <azam1976@gmail.com> wrote:

Dear Experts,

ASME Section II Part A Edition 2010

ASME SA 333/SA 333M

 

The Pipe material is ASME SA 333 Gr.6, as per clause 5.2 and Table-1 the allowable chemical element is C, Mn, P, S, Si only

As per material MTC chemical element is C (0.17%), Mn (093%), P (0.010), S (0.0010), Si (0.24), Cu(0.050%), Cr (0.12%), Ni (0.060%), Mo(0.020%), V(less than 0.004%).

 

Our query is weather above chemical element (MTC) can be accepted for ASME SA333 Gr.6.

 

Looking forward to see the comment from Mr.Pradip Goswami on above matter.

 

Thanks & Regards,

Mohd. Azam

Doha-Qatar



On Wed, Mar 13, 2013 at 3:35 PM, Azam Mohd <azam1976@gmail.com> wrote:

Dear Experts,

The below material chemical composition for ASME SA 333 Gr. 6 as per MTC

 

 

But as per ASME SA 333 Gr.6, Allowable chemical element C, Mn, P, S, Si only. Please refer ASME Section II Part A Edition 2010 clause 5.2.

 

Need your comment weather this chemical composition can be accepted. Please provide the technical clarification or code reference.

 

Thanks & Regards,

Mohd. Azam




--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 
This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...