Sunday, March 31, 2013

Re: FW: [MW:17258] Re: ASME SA 333 Gr. 6 Chemical composition

Not allowed as per SA333 /5.2 for gr 1,6,10

On 3/31/13, pgoswami <pgoswami@quickclic.net> wrote:
> Dear Azam,
>
> I missed your email in the first place. Strictly as per Clause 5.2 of SA
> 333-2010 specification addition of these alloying elements are not
> permitted. However some of the alloying elements may come from the scrap
> used for steel melting.
>
> What's the quantity involved? and what're the design requirements ?
>
> A re-check of chemistry by OES spectroscopy would be advisable. If the
> results of OES conforms to the results of manufacture's "MTR", then
> material is to be discarded.
>
> If the OES results do not pick up any of the alloying elements as
> indicated
> below, then it would be projects' discretion (i.e Client. EPC contractor
> and fabricator joint acceptance).
>
> However talk to the mill in parallel and see if replacement is available ,
> without jeopardizing manufacturing schedule.
>
>
> Pradip Goswami,P.Eng.IWE
>
> Welding & Metallurgical Specialist
>
> Ontario, Canada.
>
> Email-pgoswami@sympatico.ca <blocked::mailto:Email-pgoswami@sympatico.ca> ,
>
> pgoswami@quickclic.net <blocked::mailto:pgoswami@quickclic.net>
>
> 5.2 When Grades 1, 6, or 10 are ordered under this specification (SA 333),
> supplying an alloy grade that specifically requires the addition of any
> element other than those listed for the ordered grade in Table 1 is not
> permitted. However, the addition of elements required for the deoxidation
> of
> the steel is permitted
>
>
> _____
>
> From: materials-welding@googlegroups.com
> [mailto:materials-welding@googlegroups.com] On Behalf Of
> george.dilintas@gr.bureauveritas.com
> Sent: Saturday, March 30, 2013 9:05 AM
> To: materials-welding
> Subject: Re: [MW:17256] Re: ASME SA 333 Gr. 6 Chemical composition
>
>
> Sorry
> But which of the additional elements is used for deoxidazation?
> Usually for deoxidazation Al or Ca is used
> Best regards
> Dr Georgios Dilintas
> Authorized Nuclear Inspector
> Authorized Inspector Supervisor
> HBS Regional Technical Manager
>
>
> _____
>
> From: sajeed zaheer [sajeed7674@gmail.com]
> Sent: 03/30/2013 11:08 AM ZE4
> To: "materials-welding@googlegroups.com"
> <materials-welding@googlegroups.com>
> Subject: Re: [MW:17254] Re: ASME SA 333 Gr. 6 Chemical composition
>
>
>
> Dear Azam,
> as per sec 8 div 1 partA pg.550 para 5 chemical composition,
>
> THE ADDITION OF ELEMENT REQUIRED FOR THE DEOXIDATION OF THE STEEL IS
> PERMITTED. AND YOU CAN ACCEPT THE ABOVE MENTION MTC AS PER THIS PARAGRAPH.
>
>
> On Wed, Mar 27, 2013 at 1:53 PM, Azam Mohd <azam1976@gmail.com> wrote:
>
>
> Dear All Experts,
>
> Please provide your feedback for below query with some technical
> justification or code reference.
>
>
>
> Thanks & Regards,
>
> Mohd. Azam
>
>
>
>
> On Tue, Mar 19, 2013 at 5:09 PM, Azam Mohd <azam1976@gmail.com> wrote:
>
>
> Dear Experts,
>
> ASME Section II Part A Edition 2010
>
> ASME SA 333/SA 333M
>
>
>
> The Pipe material is ASME SA 333 Gr.6, as per clause 5.2 and Table-1 the
> allowable chemical element is C, Mn, P, S, Si only
>
> As per material MTC chemical element is C (0.17%), Mn (093%), P (0.010), S
> (0.0010), Si (0.24), Cu(0.050%), Cr (0.12%), Ni (0.060%), Mo(0.020%),
> V(less
> than 0.004%).
>
>
>
> Our query is weather above chemical element (MTC) can be accepted for ASME
> SA333 Gr.6.
>
>
>
> Looking forward to see the comment from Mr.Pradip Goswami on above matter.
>
>
>
> Thanks & Regards,
>
> Mohd. Azam
>
> Doha-Qatar
>
>
>
> On Wed, Mar 13, 2013 at 3:35 PM, Azam Mohd <azam1976@gmail.com> wrote:
>
>
> Dear Experts,
>
> The below material chemical composition for ASME SA 333 Gr. 6 as per MTC
>
>
>
>
>
>
>
> But as per ASME SA 333 Gr.6, Allowable chemical element C, Mn, P, S, Si
> only. Please refer ASME Section II Part A Edition 2010 clause 5.2.
>
>
>
> Need your comment weather this chemical composition can be accepted. Please
> provide the technical clarification or code reference.
>
>
>
> Thanks & Regards,
>
> Mohd. Azam
>
>
>
>
>
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> <mailto:materials-welding%2Bunsubscribe@googlegroups.com>
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=
> <http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk
> =anet_ug_hm> &gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups
> "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an
> email to materials-welding+unsubscribe@googlegroups.com
> <mailto:materials-welding%2Bunsubscribe@googlegroups.com> .
> For more options, visit https://groups.google.com/groups/opt_out.
>
>
>
>
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=
> <http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk
> =anet_ug_hm> &gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups
> "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an
> email to materials-welding+unsubscribe@googlegroups.com.
> For more options, visit https://groups.google.com/groups/opt_out.
>
>
> This message contains confidential information. To know more, please click
> on the following link: http://disclaimer.bureauveritas.com
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=
> <http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk
> =anet_ug_hm> &gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups
> "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an
> email to materials-welding+unsubscribe@googlegroups.com.
> For more options, visit https://groups.google.com/groups/opt_out.
>
>
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups
> "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an
> email to materials-welding+unsubscribe@googlegroups.com.
> For more options, visit https://groups.google.com/groups/opt_out.
>
>
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

FW: [MW:17257] Re: ASME SA 333 Gr. 6 Chemical composition

Dear Azam,
 
I missed your email in the first place. Strictly as per Clause 5.2 of SA 333-2010 specification addition of these alloying elements are not permitted. However some of the alloying elements may come from the scrap used for steel melting.
 
What's the quantity involved? and what're the design requirements ?
 
A re-check of  chemistry by OES spectroscopy would be advisable. If the results of OES conforms to the  results of manufacture's "MTR",  then material is  to be discarded.
 
If the OES results do not pick up any of the alloying elements as  indicated below, then it would be  projects' discretion (i.e Client. EPC contractor and fabricator joint acceptance).
 
However talk to the mill in parallel and see if replacement is available , without jeopardizing manufacturing schedule.
 

Pradip Goswami,P.Eng.IWE

Welding & Metallurgical Specialist

Ontario, Canada.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

5.2 When  Grades 1, 6, or 10 are ordered under this specification (SA 333), supplying an alloy grade that specifically requires the addition of any element other than those listed for the ordered grade in Table 1 is not permitted. However, the addition of elements required for the deoxidation of the steel is permitted



From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of george.dilintas@gr.bureauveritas.com
Sent: Saturday, March 30, 2013 9:05 AM
To: materials-welding
Subject: Re: [MW:17256] Re: ASME SA 333 Gr. 6 Chemical composition

Sorry
But which of the additional elements is used for deoxidazation?
Usually for deoxidazation Al or Ca is used
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager


  From: sajeed zaheer [sajeed7674@gmail.com]
  Sent: 03/30/2013 11:08 AM ZE4
  To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
  Subject: Re: [MW:17254] Re: ASME SA 333 Gr. 6 Chemical composition


Dear Azam,
as per sec 8 div 1 partA  pg.550 para 5 chemical composition,

THE ADDITION OF ELEMENT REQUIRED FOR THE DEOXIDATION OF THE STEEL IS PERMITTED. AND YOU CAN ACCEPT THE ABOVE MENTION MTC AS PER THIS PARAGRAPH. 


On Wed, Mar 27, 2013 at 1:53 PM, Azam Mohd <azam1976@gmail.com> wrote:

Dear All Experts,

Please provide your feedback for below query with some technical justification or code reference.

 

Thanks & Regards,

Mohd. Azam


On Tue, Mar 19, 2013 at 5:09 PM, Azam Mohd <azam1976@gmail.com> wrote:

Dear Experts,

ASME Section II Part A Edition 2010

ASME SA 333/SA 333M

 

The Pipe material is ASME SA 333 Gr.6, as per clause 5.2 and Table-1 the allowable chemical element is C, Mn, P, S, Si only

As per material MTC chemical element is C (0.17%), Mn (093%), P (0.010), S (0.0010), Si (0.24), Cu(0.050%), Cr (0.12%), Ni (0.060%), Mo(0.020%), V(less than 0.004%).

 

Our query is weather above chemical element (MTC) can be accepted for ASME SA333 Gr.6.

 

Looking forward to see the comment from Mr.Pradip Goswami on above matter.

 

Thanks & Regards,

Mohd. Azam

Doha-Qatar



On Wed, Mar 13, 2013 at 3:35 PM, Azam Mohd <azam1976@gmail.com> wrote:

Dear Experts,

The below material chemical composition for ASME SA 333 Gr. 6 as per MTC

 

 

But as per ASME SA 333 Gr.6, Allowable chemical element C, Mn, P, S, Si only. Please refer ASME Section II Part A Edition 2010 clause 5.2.

 

Need your comment weather this chemical composition can be accepted. Please provide the technical clarification or code reference.

 

Thanks & Regards,

Mohd. Azam




--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 
This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Saturday, March 30, 2013

Re: [MW:17256] Re: ASME SA 333 Gr. 6 Chemical composition

Sorry
But which of the additional elements is used for deoxidazation?
Usually for deoxidazation Al or Ca is used
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager


  From: sajeed zaheer [sajeed7674@gmail.com]
  Sent: 03/30/2013 11:08 AM ZE4
  To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
  Subject: Re: [MW:17254] Re: ASME SA 333 Gr. 6 Chemical composition


Dear Azam,
as per sec 8 div 1 partA  pg.550 para 5 chemical composition,

THE ADDITION OF ELEMENT REQUIRED FOR THE DEOXIDATION OF THE STEEL IS PERMITTED. AND YOU CAN ACCEPT THE ABOVE MENTION MTC AS PER THIS PARAGRAPH. 


On Wed, Mar 27, 2013 at 1:53 PM, Azam Mohd <azam1976@gmail.com> wrote:

Dear All Experts,

Please provide your feedback for below query with some technical justification or code reference.

 

Thanks & Regards,

Mohd. Azam


On Tue, Mar 19, 2013 at 5:09 PM, Azam Mohd <azam1976@gmail.com> wrote:

Dear Experts,

ASME Section II Part A Edition 2010

ASME SA 333/SA 333M

 

The Pipe material is ASME SA 333 Gr.6, as per clause 5.2 and Table-1 the allowable chemical element is C, Mn, P, S, Si only

As per material MTC chemical element is C (0.17%), Mn (093%), P (0.010), S (0.0010), Si (0.24), Cu(0.050%), Cr (0.12%), Ni (0.060%), Mo(0.020%), V(less than 0.004%).

 

Our query is weather above chemical element (MTC) can be accepted for ASME SA333 Gr.6.

 

Looking forward to see the comment from Mr.Pradip Goswami on above matter.

 

Thanks & Regards,

Mohd. Azam

Doha-Qatar



On Wed, Mar 13, 2013 at 3:35 PM, Azam Mohd <azam1976@gmail.com> wrote:

Dear Experts,

The below material chemical composition for ASME SA 333 Gr. 6 as per MTC

 

 

But as per ASME SA 333 Gr.6, Allowable chemical element C, Mn, P, S, Si only. Please refer ASME Section II Part A Edition 2010 clause 5.2.

 

Need your comment weather this chemical composition can be accepted. Please provide the technical clarification or code reference.

 

Thanks & Regards,

Mohd. Azam




--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 
This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Re: [MW:17254] Re: ASME SA 333 Gr. 6 Chemical composition

Dear Azam,
as per sec 8 div 1 partA  pg.550 para 5 chemical composition,

THE ADDITION OF ELEMENT REQUIRED FOR THE DEOXIDATION OF THE STEEL IS PERMITTED. AND YOU CAN ACCEPT THE ABOVE MENTION MTC AS PER THIS PARAGRAPH. 


On Wed, Mar 27, 2013 at 1:53 PM, Azam Mohd <azam1976@gmail.com> wrote:

Dear All Experts,

Please provide your feedback for below query with some technical justification or code reference.

 

Thanks & Regards,

Mohd. Azam


On Tue, Mar 19, 2013 at 5:09 PM, Azam Mohd <azam1976@gmail.com> wrote:

Dear Experts,

ASME Section II Part A Edition 2010

ASME SA 333/SA 333M

 

The Pipe material is ASME SA 333 Gr.6, as per clause 5.2 and Table-1 the allowable chemical element is C, Mn, P, S, Si only

As per material MTC chemical element is C (0.17%), Mn (093%), P (0.010), S (0.0010), Si (0.24), Cu(0.050%), Cr (0.12%), Ni (0.060%), Mo(0.020%), V(less than 0.004%).

 

Our query is weather above chemical element (MTC) can be accepted for ASME SA333 Gr.6.

 

Looking forward to see the comment from Mr.Pradip Goswami on above matter.

 

Thanks & Regards,

Mohd. Azam

Doha-Qatar



On Wed, Mar 13, 2013 at 3:35 PM, Azam Mohd <azam1976@gmail.com> wrote:

Dear Experts,

The below material chemical composition for ASME SA 333 Gr. 6 as per MTC

 

 

But as per ASME SA 333 Gr.6, Allowable chemical element C, Mn, P, S, Si only. Please refer ASME Section II Part A Edition 2010 clause 5.2.

 

Need your comment weather this chemical composition can be accepted. Please provide the technical clarification or code reference.

 

Thanks & Regards,

Mohd. Azam




--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Re: [MW:17255] Filler Required for 10Cr 3Co Material

Hi!!!!
 
For SMAW:   AWS E9018-B3,AWS E8015-B3L,AWS E9018-B3.
    GTAW :    AWS ER90S-B3

     SAW :       

BS EN SA FB 1


On Wed, Mar 27, 2013 at 2:04 PM, HITESH AGRAVAL <hitesh.agraval@gmail.com> wrote:
Dear All,

Please provide me filler can be used for 10Cr-3Co Material. Also if any body know P No. & Grade for the same. 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 



--
Thanks &Regards,
Polireddy SrinnivasaRao

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Re: [MW:17253] HPV & LPD pressure difference.

in addition to standard and specific practices of hydrostatic pressure testing, either drain or high point vent points valves (LPT, HPT) shall also be tested as per drain/vent valve specification and API standard applicable (like API 6D +) and it should be clearly mentioned in METHOD STATEMENT of HT. (1.5 times of design pressure / MAWP as required)

it may vary as per location, (on/offshore), length of vent / drain point from tapping, closed drain, material spec
 
chandrakant mohikar

 


On Thu, Mar 28, 2013 at 6:07 AM, Jawed Anwar <jawed81@gmail.com> wrote:
DEAR EXPERTS
  i have one query that during hyedro test where should be the pressure guage show the high pressure value at high point vent or low point drain ,and why ?
 
Thanks & best regards.
Mohammad Jawed Anwar .
(welding inspector)
Mob no #  +966569799776.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Friday, March 29, 2013

Re: [MW:17252] HPV & LPD pressure difference.

Dear Jawedji,

From the subject of  fluid mechanics at lower level water pressure is very high due to water head created  between upper level and lower level.it can be calculated as per given below:

Head loss=R*g*H

Where R=Density of fluid.
          g=gravity.
          H=head created between lower level and upper level.


From: Ranendra Chakraborty <ranendrac6@gmail.com>
To: materials-welding@googlegroups.com
Sent: Friday, 29 March 2013 3:34 PM
Subject: Re: [MW:17251] HPV & LPD pressure difference.

Dear Jawed,
The pressure at LPD is higher and the difference is due to the pressure of the height of water column.
 
Regards,
Ranendra

On Thu, Mar 28, 2013 at 8:59 AM, Rana Vikas <vhrana@gmail.com> wrote:
Lower level i.e drain side pressure found higher compare to vent i.e on top side. This difference in pressure due to gravity level.

With Regards,
Vikas Rana



On Thu, Mar 28, 2013 at 6:07 AM, Jawed Anwar <jawed81@gmail.com> wrote:
DEAR EXPERTS
  i have one query that during hyedro test where should be the pressure guage show the high pressure value at high point vent or low point drain ,and why ?
 
Thanks & best regards.
Mohammad Jawed Anwar .
(welding inspector)
Mob no #  +966569799776.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 


Re: [MW:17251] HPV & LPD pressure difference.

Dear Jawed,
The pressure at LPD is higher and the difference is due to the pressure of the height of water column.
 
Regards,
Ranendra

On Thu, Mar 28, 2013 at 8:59 AM, Rana Vikas <vhrana@gmail.com> wrote:
Lower level i.e drain side pressure found higher compare to vent i.e on top side. This difference in pressure due to gravity level.

With Regards,
Vikas Rana



On Thu, Mar 28, 2013 at 6:07 AM, Jawed Anwar <jawed81@gmail.com> wrote:
DEAR EXPERTS
  i have one query that during hyedro test where should be the pressure guage show the high pressure value at high point vent or low point drain ,and why ?
 
Thanks & best regards.
Mohammad Jawed Anwar .
(welding inspector)
Mob no #  +966569799776.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Re: [MW:17249] Distance between two L-Seam

Such stuff are referenced in corresponding project specifications, as these can not be generalised.

ವಂದನೆಗಳೊಂದಿಗೆ / Best regards,

Nandesh Kumar A

Abu Dhabi, UAE

P.S. : Please don't print this e-mail unless you really need to.


--- On Thu, 28/3/13, Himanshu Patel <absgpatel@gmail.com> wrote:

From: Himanshu Patel <absgpatel@gmail.com>
Subject: Re: [MW:17246] Distance between two L-Seam
To: materials-welding@googlegroups.com
Date: Thursday, 28 March, 2013, 5:41 AM

Hello To ALL,
 
This clause applicable to Pressure Vessel, What about PIPING can any one suggest for piping as per (API 1104, B31.4, B31.3 or B31.1).
 
Thanks.
 

On Thursday, June 14, 2012 11:56:49 AM UTC+4, saravanan sornam wrote:
Hi Guru,
 
You can find in ASME VIII Div. I, UW-9 (d).
 
(d) Except when the longitudinal joints are radiographed
4 in. (100 mm) each side of each circumferential welded
intersection, vessels made up of two or more courses shall
have the centers of the welded longitudinal joints of adjacent
courses staggered or separated by a distance of at
least five times the thickness of the thicker plate.
 
Hope it is Ok for U...
 
Cheers,
Sarav,
Korea

On Thu, Jun 14, 2012 at 12:24 PM, Gurunath.Hanamar <guru...@gmail.com> wrote:

Dear all,
I know that 100mm is permissble distance between two consecutive longitudinal seams but, can any one confirm minimum distance between two longitudinal seams should be mantained. Kindly mention ASME clause.

Thanks &Regards
Gurunath Hanamar

--
To post to this group, send email to material...@ googlegroups.com
To unsubscribe from this group, send email to materials-weld...@ googlegroups.com
For more options, visit this group's bolg at http://materials-welding. blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Thursday, March 28, 2013

Re: [MW:17250] Unlimited thickness welding test how many test coupons required ?

QW-453

PROCEDURE/PERFORMANCE QUALIFICATION THICKNESS LIMITS AND TEST

 

NOTES:

(1) The qualification test coupon shall consist of base metal not less than 6 in. (150 mm)

6 in. (150 mm). The weld overlay cladding shall be

a minimum of 1

12 in. (38 mm) wide by approximately 6 in. (150 mm) long. For qualification on pipe, the pipe length shall be a minimum

of 6 in. (150 mm), and a minimum diameter to allow the required number of test specimens. The weld overlay shall be continuous around

the circumference of the test coupon. For processes (performance qualification only) depositing a weld bead width greater than

12 in. (13 mm)

wide, the weld overlay shall consist of a minimum of three weld beads in the first layer.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Re: [MW:17248] Distance between two L-Seam

Dear Mr. Himanshu,

As per B 31.3 seam to seam minimum distance is given as 4 times thickness but B 31.3  haven't mentioned L seam to L seam staggering. Means can be weld without staggering.

ವಂದನೆಗಳೊಂದಿಗೆ / Best regards, 
Gurunath Hanamar


On Thu, Mar 28, 2013 at 11:11 AM, Himanshu Patel <absgpatel@gmail.com> wrote:
Hello To ALL,
 
This clause applicable to Pressure Vessel, What about PIPING can any one suggest for piping as per (API 1104, B31.4, B31.3 or B31.1).
 
Thanks.
 

On Thursday, June 14, 2012 11:56:49 AM UTC+4, saravanan sornam wrote:
Hi Guru,
 
You can find in ASME VIII Div. I, UW-9 (d).
 
(d) Except when the longitudinal joints are radiographed
4 in. (100 mm) each side of each circumferential welded
intersection, vessels made up of two or more courses shall
have the centers of the welded longitudinal joints of adjacent
courses staggered or separated by a distance of at
least five times the thickness of the thicker plate.
 
Hope it is Ok for U...
 
Cheers,
Sarav,
Korea

On Thu, Jun 14, 2012 at 12:24 PM, Gurunath.Hanamar <guru...@gmail.com> wrote:

Dear all,
I know that 100mm is permissble distance between two consecutive longitudinal seams but, can any one confirm minimum distance between two longitudinal seams should be mantained. Kindly mention ASME clause.

Thanks &Regards
Gurunath Hanamar

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

[MW:17245] Re: WPS with PWHT below the lower transformation temperature

dear all,

I under stand B31.3 so now can i make WPS up to 649ºC without requalification of original WPS .

regards,
mohd.

On Saturday, March 23, 2013 10:20:32 AM UTC+3, mohd wrote:

Dear all,

WPS details as per ASME IX  Design Code :B31.3

1) GTAW + SMAW (3mm+ 24mm)
2) Material API 5L x52 Thk : 26.97
3) PWHT 600 +/-20  Time : 1Hr  20min
4) No impact.
 
Can I Re Write WPS with Temperature  670+/-20 as per As per QW-407.1 a (2) ? ( up to below Lower transformation no need re qualification )

Need expert Opinion.

QW-407 Postweld Heat Treatment
QW-407.1 A separate procedure qualification is
required for each of the following:
(a) For P-Numbers 1 through 6 and 9 through 15F materials,
the following postweld heat treatment conditions
apply:
(1) no PWHT
(2) PWHT below the lower transformation temperature )



Regards,
mohd.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Re: [MW:17246] Distance between two L-Seam

Hello To ALL,
 
This clause applicable to Pressure Vessel, What about PIPING can any one suggest for piping as per (API 1104, B31.4, B31.3 or B31.1).
 
Thanks.
 

On Thursday, June 14, 2012 11:56:49 AM UTC+4, saravanan sornam wrote:
Hi Guru,
 
You can find in ASME VIII Div. I, UW-9 (d).
 
(d) Except when the longitudinal joints are radiographed
4 in. (100 mm) each side of each circumferential welded
intersection, vessels made up of two or more courses shall
have the centers of the welded longitudinal joints of adjacent
courses staggered or separated by a distance of at
least five times the thickness of the thicker plate.
 
Hope it is Ok for U...
 
Cheers,
Sarav,
Korea

On Thu, Jun 14, 2012 at 12:24 PM, Gurunath.Hanamar <guru...@gmail.com> wrote:

Dear all,
I know that 100mm is permissble distance between two consecutive longitudinal seams but, can any one confirm minimum distance between two longitudinal seams should be mantained. Kindly mention ASME clause.

Thanks &Regards
Gurunath Hanamar

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

[MW:35633] IP Joint

Hello experts, I would like to know what is IP joints in piping(31.3)?  Regards Saurabh -- https://materials-welding.blogspot.com/...