RE: [MW:12750] RT density

Referring to ASME V, Art. 2 T-282.1 & 282.2 I understand it to read that the “area of interest” (and IQI) can not exceed 2.0 to 4.0.  What is your area of interest, is it between the location markers, is it the weld, heat affected zone, base metal, how much “area of interest” do you have?  I have one level III that has said “area of interest” is between position/location markers, while other Level III’s have said it’s the area that you are interested in.  Spelling it out in the Procedure would be ideal.   

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of meisam shokri arfaei
Sent: Friday, October 21, 2011 1:15 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:12737] RT density

 

Dear Pankaj,

Any NDT related work shall have a written procedure. These procedures may be in accordance with one or more codes or standards which support the user for some special works. In those procedures special situation for the work shall be defined. the first place that you have to search for such information about overlap of films is in written procedures.

But in general, there is a qualified range of film density that the interpreter can evaluate radiographic film in this range. The overlap shall be in such a way that each part of the film that is out of this range (usually lesser in density) repeats in next shoot within the in-range film density.

 

Regards

On Thu, Oct 20, 2011 at 10:38 PM, Nandesh Kumar <nandeshkumar@rocketmail.com> wrote:

Dear Pankaj,

 

Film overlap is given only for identification purpose that the same weld is continued.

 

Dont measure the density on the overlapped lighter area. Measure the density on un overlapped area of the previous film.

 

Its a general knowledge and no code says anything about that, as far as I know.

 

Nandeesh

 



--- On Thu, 20/10/11, pankaj.kolhe15 <pankaj.kolhe15@gmail.com> wrote:


From: pankaj.kolhe15 <pankaj.kolhe15@gmail.com>
Subject: [MW:12728] RT density
To: "pgoswami" <pgoswami@quickclic.net>, "materials-welding" <materials-welding@googlegroups.com>
Date: Thursday, 20 October, 2011, 3:09 PM

 

Dear sir,
what is the density requirement at overlapped area , if the two films
got overlapped
for gamma rays and where it is written

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.




--

M. Shokri Arfaei

International Welding Engineer (IWE)

ASNT NDT Level III

ERI Metallurgy Lab. Manager

Tel: +98-21-66283696

Fax: +98-21-66283693

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



DISCLAIMER: The information contained in this e-mail may be confidential and is intended solely for the use of the named addressee. Access, copying or re-use of the e-mail or any information contained therein by any other person is not authorized. If you are not the intended recipient please notify us immediately by returning the e-mail to the originator.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...