Dear abdul,
                if the welder qualifies in 6G position to maximum thickness (more than 13mm). that welder is qualified in 4G position on plate also upto maximum thickness.

On Sat, Jul 30, 2011 at 9:09 AM, arvinda shan <arvindashan@gmail.com> wrote:
Dear Mr.Abdul,
 
6G is for position. If he qualifies in 6G position, he can do welding in any position . Reference.....SecIX- QW-461.9
 
For thickness, upto 13 mm thickness , he qualifies 2T. Beyond 13 mm , unlimited thickness.  Reference..... Sec IX -QW-452.1(b)
 
Regards
 
Arvinda.

On Fri, Jul 29, 2011 at 8:19 AM, Suresh <bobsuresh24@gmail.com> wrote:
Mr.Abdul ,
 
Your query is not clear ....Thickness qualification is  depends on weld cupon thickness , not depends on  Position ...
 
If the welder is qualified 6G Position then he can qualify any position but not any thickness..
 
Normally Sex IX , 2T is welder for thickness range qualification
 
Suresh

On Thu, Jul 28, 2011 at 7:32 PM, abdul khan <abdul_khan2010@yahoo.co.in> wrote:
Dear Experts ,
 
If the wleder is  qualifide for 6G test , can he weld the plate of  unlimited thickness ?
or he needs to Qualify 4G test to weld unlimited thickness of plate ?
 
wether the 6G welder is sapose to weld only pipes.
 

awaiting for  welding experts valueable  suggestions ..........

 

Regards

ABDUL JABBAR KHAN

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Thanks  & Best Regards,

Suresh

Mobile No: 91-92 92 905 905


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
THANKS & REGARDS
 
KALYAN VVV
WELDING ENGINEER
HYDERABAD
Mob.NO- 09885273257

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...