Thursday, April 7, 2011

[MW:10625] Re: replacement of UT by RT

Dear Asad,

The examination either RT or UT, I have the following view point.
- As per ASME Section VIII-1 & 2, RT is only the mandatory requirement
& UT in accordance with UW-53 may be substituted for radiography for
the final closure seam of a pressure vessel if the construction of the
vessel does not permit interpretable radiographs in accordance with
Code requirements. The absence of suitable radiographic equipment
shall not be justification for such substitution
- Why UT is not mandatory, the fracture mechanics gives some details
as per this many conditions rejected by RT do not affect in-service
integrity. With RT the worst-case depth must be assumed, through wall.
But not all cracks need repair
- Similarly for RT examination geometry is important factor, sometimes
it is impossible to interpret the radiograph like in set-in or set on
type nozzle to shell joints.
- RT sometimes cannot interpret side wall lack of fusion, cold laps &
laminations in base metal, which can be better seen in UT.

Regards

Jaspal Singh
Quality Assurance
ISGEC-Yamunanagar
09996624244

On Apr 7, 12:49 pm, asad azmi <azmiasada...@gmail.com> wrote:
> Dear ALL,
>
> Can we replace UT by RT for any weld joint.
>
> can somebody expalin me advantage/disadvantage of UT over RT.
>
> Thanks and Regards
>
> Asad Azmi

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...