Skip to main content

[MW:690] Re: 688] Re: PMI TESTING OF SS 304L

DEAR Mr. RAGHURAM,
 
BUT SPARK EMISSION WHAT WE ARE ADOPTING HERE IS ARGON BASED AND MANY TIMES I FOUND PURITY OF ARGON IS NOT ENSURED. HENCE I AM RELUCANT TO GO FOR SPARK EMISSION FOR PMI OF LOW CARBON SS.
 
YOUR VIEWS PLEASE.
 
REGARDS,
 
S.N.DAVE

"Bathula Raghuram (Mumbai - PIPING)" <R.Bathula@ticb.com> wrote:
Why not? Infact only sprak emission method can detect C, as these are not portables instruments maneuvering at construction sites is very difficult
Both Arc met and PMI Master (see the other post by Mr Nadig, WAS is from oxford instruments, US) are gas based, where the principle of Spectro isort is quite different, it neither use Argon nor X-ray source.
 
However take care while using spark emission on lighter wall components
 
 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of shailesh dave
Sent: Monday, March 24, 2008 2:58 PM
To: materials-welding@googlegroups.com
Subject: [MW:688] Re: PMI TESTING OF SS 304L
 
DEAR Mr. RAGHURAM,
 
THANKS FOR THE REPLY. JUST ADVISE ME IS IT RECOMMANDED TO USE SPARK EMISSION TECHNIQUE ON SS 304L MATERAIL FOR PMI.
 
AWAITING YOUR REPLY.
 
REGARDS,
 
S.N.DAVE

"Bathula Raghuram (Mumbai - PIPING)" <R.Bathula@ticb.com> wrote:
Probably spectro isort by Amtek can detect C, (thou I have not used it), you can try at www.spectro.com
 
Also Arcmet930 by Metorex can detect C
 

From: shailesh dave [mailto:snd2988@yahoo.com]
Sent: Monday, March 24, 2008 2:07 PM
To: materials-welding@googlegroups.com
Subject: PMI TESTING OF SS 304L
 
DEAR MEMBERS,
 
CAN ANYBODY TELL ME WHAT TECHNIQUE SHOULD BE USE TO PERFORM PMI OF SS304L. SINCE CARBON ANALYSIS IS VERY VERY IMPORTANT.
 
REGARDS,
 
S.N.DAVE
 
QA/QC MANAGER - TATA PROJECTS,
 
IWPP -III, SHUIBAH, SAUDI ARABIA


Be a better friend, newshound, and know-it-all with Yahoo! Mobile. Try it now. --~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .