[MW:655] Re: Consumables for API 5L GR X65

 
 
De: materials-welding@googlegroups.com
Para: materials-welding@googlegroups.com
Copia: piping_valves@yahoogroups.com
Fecha: Fri, 7 Mar 2008 14:18:16 +0530
Asunto: [MW:654] Consumables for API 5L GR X65

You can use EX010-P1 (Pipeline) Electrodes. These  electrodes have been designed primarily for welding typical high-strength, pipe butt joints in the vertical welding position with downward or upward progression.

This combination is best suited for achieving full penetration and radiographic quality for the downhill welding of butt joints when the axis of the pipe is in the horizontal position.

 


From: dharmesh arvadia [mailto:dharmeshedc@yahoo.co.in]
Sent: Friday, March 07, 2008 1:04 PM
To: materials-welding@googlegroups.com
Cc: piping_valves@yahoogroups.com
Subject: API 5L GR X65

 

 

Dear group.
 
   Kindly advise me which electrod i can use for pipe to pipe welding 
for material API 5L GR X65
   WITH REASON.
 
   Best regards.
   Dharmesh Arvadia.
   You can use in process SMAW E-8010, Down Hill or Up Hill pending  if is API 1104 or ASME B31.3 I am using in Gas Plant
GTAW/SMAW ER-70S-X/E-8018G
 
 



--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...