Mr. Pal.
E 8018- B8 / E 8015 –B8 / E 8016 – B8 Low Alloy Steel Electrodes.
All above electrodes ( formally 505 family) have typical chemistry of
9 Cr & 1 Mo. And well suitable to weld ASTM grades: A182-F9, A336-F9,
A199-T9, A200-T9, A213-T9, A335-P9, A369-FP9, A426-CP9, A217-C12, and A387- Gr9. Idea for high pressure hydrogen service.
Simply put the main difference between above categories are:
8015-B8 = Low-hydrogen sodium coating and used with DCEP
8016-B8 = Low-hydrogen potassium coating used with DCEP or AC
8018-B8 = Low-hydrogen potassium, iron powder coating used with DCEP or AC
Procedures may vary with change in position, base metals, filler metals, equipment and other changes. Preheat and post-heat recommended for all.
SPECIFICATIONS:
ANSI/AWS A5.5 E8015-B8 , E8016-B8 , 8018-B8
ASME SFA A5.5 E8015-B8 , E8016-B8 , 8018-B8
(Formerly AWS A 5.4, Class E505-15 , E505-16 , N/A FOR -18)
Sridhar.
From: Biplab Pal <biplab.mech@googlemail.com>
To: materials-welding <materials-welding@googlegroups.com>; JALADHAR JENA <jdjena2006@yahoo.co.in>; Pinaki Boxi <boxi.pinaki@gmail.com>; chandan.majumdar <chandan.majumdar@sgs.com>
Sent: Saturday, 5 January 2013 11:20 AM
Subject: [MW:16440] Difference between the electrode E8018 B-8 & E8015 B-8
Dear Experts,
Can any body differentiate between the electrodes E8018 B-8 & E8015 B-8, and the difference of applicable areas.
--
-- Can any body differentiate between the electrodes E8018 B-8 & E8015 B-8, and the difference of applicable areas.
--
Thanks & Regards
Biplab Pal
Welding Inspector
Biplab Pal
Welding Inspector
E-mail: biplab.mech@gmail.com
Information in this email and any attachments is confidential and intended solely for the use of the individual(s) to whom it is addressed or otherwise directed. Please note that any views or opinions presented in this email are solely those of the author and do not necessarily represent those of the Company. Finally, the recipient should check this email and any attachments for the presence of viruses. Myself accepts no liability for any damage caused by any virus transmitted by this email.
Information in this email and any attachments is confidential and intended solely for the use of the individual(s) to whom it is addressed or otherwise directed. Please note that any views or opinions presented in this email are solely those of the author and do not necessarily represent those of the Company. Finally, the recipient should check this email and any attachments for the presence of viruses. Myself accepts no liability for any damage caused by any virus transmitted by this email.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
No comments:
Post a Comment