Re: [MW:27762] AWS D 1.1 interpretation on Increase in Preheat / Interpass temperature

Increase in preheat temperature is not essential variable; decrease in preheat temperature is essential variable. 
Increase in inter-pass temperature is supplementary essential variable (applicable only when notch toughness is required).  
Any client who claims increase preheat temperature is essential variable does not understand the code requirement.

On ‎Wednesday‎, ‎2‎ ‎May‎ ‎2018‎ ‎04‎:‎58‎:‎49‎ ‎WAT, N VENKATESWARA PRASAD <weldengr.velosi@gmail.com> wrote:


Dear Experts,

We have received a comment on Increase in Preheat temperature greater than 56°C is essential variable as per AWS D.1 from our client.

My interpretation is the increase in 56°C is applicable only for inter pass temperature.  The details are as given below. 

 

PQR   Test coupon thickness        :  30 mm

PQR   Preheat temperature          :  30°C

PQR Inter pass temperature        :  173°C

 

Job Thickness                                  : > 38 mm  to 65 mm  ( As per Table 3.3)

Preheat temperature                    :  110°C

Inter pass temperature                 :  220°C

MDMT                                               :  -40 °C

 

As per AWS D 1.1  Table 4.6  Point no. 7   an increase more than 56°C in max preheat or interpass temperature is essential variable  for CVN testing applications.

 

Based on the above clause, the client is insisting that the Qualified Range for  thickness in WPS shall be restricted to 38 mm as the preheat is increased from 30°C to 110°C which is not acceptable .

 

Please provide me if you any interpretation on it from AWS.

Regards

Prasad

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35614] Re: SS FILLER

dear , pl check A number and Gas composition use for ss cant be sutibale same % for duplex., u need to qualified with aditional testing of f...