Re: [MW:24189] Hardness Of P-91 Material

Dear Mr.Kumar

Normally 760 C with 4 hours holding time required to get a hardness value.But always follow your WPS requirements and client specifications. 


Thanks & Regards
Nareshkumar Subramanian




From: Mohammad Saquib <saquibqaqc@gmail.com>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Sent: Saturday, January 30, 2016 9:20 AM
Subject: Re: [MW:24188] Hardness Of P-91 Material

Dear Kumar,
you have to do re PWHT 2 hours holding time at 725 degree centrigrade  make sure the heating & cooling rate is not more than 100 degree

On Sat, Jan 30, 2016 at 7:59 AM, pradip kumar Sil <pradipsil@gmail.com> wrote:
Dear Everybody,

Some of our P-91 Joints( Weldment) are coming hardness value around 300HB in the HRSG Unit.
 Joints thickness is 18 mm & 20 mm & we did PWHT 2 hours holding time at 710 degree centrigrade also we did 150 degree heating rate ,120 degree cooling rate.

Can you pls suggest us this hardness value  is acceptable in the HRSG unit. If not pls suggest me how to recover.
Regards,
Kumar
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAB%3DAs8mJXj9twE50bbG4-%2Bb-_35XPHeuAZ97xUD5n1Aq7TR21Q%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADA7dVUEpQs_-naFazHR%2BWeV2bEY2dyDTYT%2B823kXKCSyxpSFA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.


No comments:

[MW:35748] Re: PQR- Chemical testing requirements

As answered by everyone, chemical is not required. Notwithstanding, please note that A-No. which denotes weld metal chemical composition is ...