Tuesday, January 19, 2016

Re: [MW:24135] Ferrite No. in Austenistic stainless steel weld overlay in FCAW process

You have not mentioned about no. of layers build up. Is it two or three.

With two layer deposit, the ferrite  could be more.

Also check on a typical SS or CS plate the ferrite content of weld metal as per SFA 5.4 

That may give an idea about filler wire..

Weld parameters like Amps, Voltage and stick out used is also important.

C Sridhar.

Mobile nos: 0 94449 71097, 0 7406 326326, 0 94445 21267.


'Life is like cycling. To keep the balance, you have to keep on going'




 




From: "george.dilintas@gr.bureauveritas.com" <george.dilintas@gr.bureauveritas.com>
To: Bhatt Purvin <materials-welding@googlegroups.com>
Sent: Sunday, 17 January 2016 1:11 PM
Subject: Re: [MW:24119] Ferrite No. in Austenistic stainless steel weld overlay in FCAW process

High dilution rate might be a reason

Sent from my BlackBerry 10 smartphone.
From: Bhatt Purvin
Sent: Σάββατο, 16 Ιανουαρίου 2016 - 17:44
To: Materials & Welding
Reply To: materials-welding@googlegroups.com
Subject: [MW:24106] Ferrite No. in Austenistic stainless steel weld overlay in FCAW process

Hello,

I find it bit strange to receive Ferrite no. above 8 or up  to 11 some times, while using FCAW weld overlay on CS surface. What are the reasons behind these. 
My requirement is 3 to 8 % only. 
Can  I have any solution for this ? .
 PWHT  will be there in my job. 
What should I do to restrict up to 8 % only, with same process.  

Warm Regards
Purvin Bhatt 
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/075922ad-610d-4296-b6a6-b04d12b687e0%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/OF08C19F9F.811FF097-ONC1257F3D.002A4897-1453016511099%40LocalDomain.
For more options, visit https://groups.google.com/d/optout.


No comments:

Re: [MW:35737] Bend Test and Tensile Test failed for ET45 Micro Welded Coupon

Hi As its %elongation is very low  Better try buttering on jt surrace with ductile consumable like pure Ni i. E Ni1 And later weld jt with c...