Yes the same PQR can be used. Please go through QW 404.12 part e of Section IX.
Regards,
Anup
On 11 Sep 2015 06:50, "Raghuram Bathula" <raghurambathula@gmail.com> wrote:
-- No, you need to follow your code of construction and support with new PQR qualified at or below MDMT--On 11 September 2015 at 09:12, Mahesh Mirje <mahesh.mirje41@gmail.com> wrote:Hi expert's,
I have PQR with electrode E7018, AND IMPACT tested at -30deg. Lets say Observed energy values 20J
Can I make wps with E7018-1, FOR IMPACT REQUIRMENT at -45 deg.required energy values 20j,
AS per ASME weld metal produced by 7018-1, will provide 20j at -45 deg.
And HAZ ENERGY VALUES CAN BE CONTROLLED BY RESTRICTING HEAT INPUT.
Pls, clarify can I prepare wps for 7018-1 at -45 by restricting heat input as same used in 7018 PQR.
Regards
Mahesh
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADxVubnJSKpehomULf6bXi%2Bv0%2BuKQesPQX2vT8KNC_YYacnnhw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJsQutYpcSXWVq8afZqf51DPjzznrojzQW9t1vfgwu5jtbMiCQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
No comments:
Post a Comment