Re: [MW:23101] Required clarification to read Rounded indications according to ASME SEC-VIII

There is table 4-1 which shows the acceptance limits regarding the type of rounded indications (random or isolated) by giving some examples and the relationship with the thickness. Generally in dissimilar thicknesses, the thinner part should be the criteria for decision (it is mentioned in 4-2-c).

So the max. dimension for rounded indication is 0.79mm for random, and 1.07mm for isolated indications regarding to your thinner thickness, 3mm. Please read 4-3 carefully for more details. 

Also Fig. 4-1 & 4-2 guide you about permissible length of indications (and not about size and number of indications).

In addition you can use fig. 4-3 for typical size, number and distribution of indications. Keep in mind that this figure is just a sample based on previous criterias and drawn for thicknesses between 3 to 6mm.

Regards

On Wed, Apr 15, 2015 at 8:00 AM, Kanikumar Kumar <kanikumar1989@gmail.com> wrote:

Dear Sirs,

I have some doubt regarding rounded indication (defects) in weld metal.

How much porosities (Numbers with size) are allowed in 3mm to 6mm material thk. According to ASME –VIII, Div-1 (Appendix 4)…

Because, In Appendix 4, FIG 4-3, lot of porosities are showed. So please Guide me.

 

Also suggest me how to read the standard with respect to Appendix-4.

 

I am waiting for your reply in this regards.

 

Thanks & Regards,

K.KANIKUMAR.


--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACZz93D6agh%3Ds56KR86JpuhQTC04QsmSt5or%2B1GSJcowmNXBMg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.



--
M. Shokri Arfaei
ISA-ISTS - Metallurgy Lab. Manager
ASNT NDT Level III
International Welding Engineer

Tel.: +98 21 66282127
Fax: +98 21 66282779
Mob.:+98 912 1394023




--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAC8uMttx0gEUdcr4BNfbww1rA6ECBLk70j4fd1fqVi_H0b%3DVbw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...