Hello Azam,


Meeting the acceptance criteria of ASTM A923 Method C for weldments in as welded condition is HIGHLY IMPOSSIBLE.


The intention of doing ASTM A 923 Method C on DSS/SDSS material is to detect the formation of detrimental intermetallic phases during manufacturing, i.e. to ensure how effectively the SOLUTION ANNEALING heat treatment is carried out by the manufacture.


Of course, if the weldments are subjected to SOLUTION ANNEALING then the requirements can be meet, but lot of practical difficulties are there in doing so at site conditions!!.


During welding we cannot avoid formation of INTERMETALLIC PHASES completely , because of slow cooling from higher temperatures, particularly  in multiple pass welding i.e in thick sections the percentage of intermetallic  phase formed will high when compared with thin sections.


But you can convince the client, by request for a technical deviation; you can substantiate the deviation by putting forward the following points.      


  1. Successful Impact test results, (Intermetallic phases deteriorate the toughness of the material )
  2. Successful Pitting corrosion test as per ASTM G48 Method A ( without any pitting on the test sample)
  3. Delta Ferrite Count within acceptable  limits,
  4. Hardness values within limits as per NACE requirements.


Regards,

On Mon, Oct 6, 2014 at 6:11 PM, Mohd Azam <azam1976@gmail.com> wrote:

Dear Experts,

Pls share your experience on super Duplex Stainless steel weld:

We run PQR for SDSS material UNS S32750 Pipe to Pipe Single “V ”butt weld, All the testing result in line with requirement like Tensile, Hardness, Macro,  Ferrite to Austenitic ratio, ASTM G48 but ASTM A923 Method C testing is not meeting the requirement

 

Acceptance Values

20.1 The corrosion rate is calculated in accordance with the

weight loss and total surface area (see Note 5). Unless

otherwise specified, the calculated corrosion rate shall not

exceed 10 mdd (see Note 6).

NOTE 5—The corrosion rate is calculated in accordance with the

following: corrosion rate (mdd)

= weight loss (mg)/[specimen area (dm2) × time (days)]

 

Even if sample will meet the requirement of ASTM G48 and Shell DEP 30.10.6018-Gen. it will not pass ASTM A923 Method C. ASTM A923C requirement is looking likemore stringent compare to ASTM G48.We prepare sample size 50 mm*10mm*thickness (3.4 mm). Pls share your expertise.

 

Thanks & Regards,

Mohd. Azam

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...