AN EXAMPLE
 
DISHED END FORMING
 
   
* Dished plate thickness  t = 6 mm  
Knuckle  radius = 150 mm  
Mean radius Rf = 150 +6/2 = 153 mm  
Original center line radius  R0= Infinity Flat Plate
%   Extream fiber elongation = ( 75 t /Rf)x(1-Rf/R0)               = (75x6/153)x(1-153/Infinity)
%   Extream fiber elongation    ( Dished end formation ) 2.94 <  20%  
As per table UHA-44 max fibre elongation permitted for 304 material is 20% hence Post fabrication heat treatment is not required


On Tue, Apr 22, 2014 at 11:26 AM, Sandeep Maan <sandeepmaan@altechinfra.com> wrote:
Dear Expert Please let me know  how to calculate fibre elongation for dish as per sec VIII Div. I

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35754] interpration

  Interpretation #: BPV IX-18-34  Record Number: 18-771  Subject Description: SC IX; QW-401.1 and QW-403.6 - Thickness Range Qualified for I...