Re: [MW:20618] API 650 - Impact acceptance criteria for A516 Gr.60

Mr. George Dilintas,
Thank you for your response.
OK. Understood. The plates are normalized, so it is group IIIA.
But even though Fig. 4-1b says that impact test is not necessary, according to 9.2.2.4, impact test of weld metal shall be made for all welding procedures when DMT< -7 ºC (20 ºF) which means, I believe, that impact teste shall be done.
If so, where are the minimun values?
Best Regards,
 
Dalton Gonçalves
Mechanical Engineer

Em quinta-feira, 17 de abril de 2014 05h33min26s UTC-3, George Dilintas escreveu:

you misinterpret 9.2.1.3.
You should at a 1st instance check if you can exempt your plates from impact testing using the figures 4-1a/4-1b.
According to the table 4-4b A516-60 is Group III if not normalized or IIIA if normalized.
Practically, according to Fig. 4-1b above -40oF you can use this material without impact testing

    best regards

    Dr. Georgios Dilintas

    Authorized Nuclear Inspector
    Authorized Inspector Supervisor
    API 510 Inspector

    I&F REGIONAL TECHNICAL MANAGER
    BUREAU VERITAS HELLAS

    Tel: +30 210 40 63 113/4
    Fax: +30 210 40 63 118
    Cell: +30 69 44 64 62 04
    (See attached file: Dilintas_George.vcf)

Inactive hide details for Dalton Gonçalves ---17/04/2014 02:35:02---A tank will be built from ASTM A516 Gr. 60. and under the rDalton Gonçalves ---17/04/2014 02:35:02---A tank will be built from ASTM A516 Gr. 60. and under the rules of API  650/2013.

From: Dalton Gonçalves <dalton.g...@gmail.com>
To: material...@googlegroups.com
Date: 17/04/2014 02:35
Subject: [MW:20607] API 650 - Impact acceptance criteria for A516 Gr.60
Sent by: material...@googlegroups.com




A tank will be built from ASTM A516 Gr. 60. and under the rules of API 650/2013.
The design temperature is 0 ºF.
The welding of horizontal shell joints will be done by SAW.
There is impact requirement for weld metal, according to 9.2.2.4 + 4.2.10.3.

The point is that ASTM A516 is included in QW-422 and according to 9.2.1.3, it is not possible consider this material as P1. Therefore, I believe it is not possible to use the values described in 9.2.2.5.

If so, where are the minimum values for impact test?

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-welding+unsubscribe@googlegroups.com.
For more options, visit
https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...