Tuesday, January 29, 2013

RE: [MW:16624] MAGNETIC CHECK

David,
 
Austenitic stainless  steel weld metals should contain some nominal amount(4-7%) of delta -ferrite to prevent hot cracks. This requirement is approximately 6% for SS 316L. Ferrite being magnetic would cause residual magnetism in the weld, and magnets would stick  if one probes the weld with the  same . Note  this magnetic force may not be very strong.
 
One may experience  the  same level of residual magnetism in 316L base  metals, if it undergoes any  cold-work(reduction).
 
Thanks.
 
P.Goswami, P.Eng

 

From: David.Chan@Exterran.com
To: materials-welding@googlegroups.com
Date: Mon, 28 Jan 2013 13:27:40 +0800
Subject: [MW:16610] MAGNETIC CHECK

Hi Experts,

We have an issue where the Customer is going around on the a stainless steel (S316L) using a potable to check on the materials and welds

 

He has checked on some areas near the weldment where there is a force of attachment and the magnet is still sticking to the area

The magnet drops off when the magnet is moving away from the weldment

 

I request for a technical understanding to clarify with the customer

 

Appreciate your kind assistance  

 

Thank you

Best Regards

 

David Chan

 

Republic of Singapore


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...