Wednesday, January 23, 2013

[MW:16577] RE: 16574] ASTM A516 Gr.70 normalizing

See 5.1 and 5.2 of the A516 specification.

 

Anything less than 1.5 inches thick is usually as rolled and anything above 1.5 inches thick is required to be normalized.

 

If you need low temperature impacts and the material thickness is less than 1.5 inches, you should specify that the material be normalized.

 

Heat treatment should be stated on CMTR.

 

John A. Henning

Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of M2M
Sent: Tuesday, January 22, 2013 8:47 PM
To: materials-welding@googlegroups.com
Subject: [MW:16574] ASTM A516 Gr.70 normalizing

 

 

Dear All

 

I need to know how can understand that ASTM A516 Gr.70 is normalized or not?

 

Somebody told me:

 “according to clause 5.3 of ASTM A516 standard (attached), when we apply charpy impact test on a material and it pass the impact test successfully, we can say the material is surly normalized but if the material can’t pass the impact test, we shall apply metallographic test to understanding if the material is normalized.

 

And somebody said me:

“we have just 1 way to know that is the material normalized or not. And its metallographic test.”

 

M. Farhang

 

 

 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...