Re: [MW:12193] 42CrMo4 ( SAE 4140 ) Welding

Dear Sinan,
I have such an experience. I did such welding with AWS A5.5 - E8018-B2. Other parts of the process which you mentioned in your post are mandatory to have a good weld.

On Thu, Aug 11, 2011 at 9:56 AM, Sinan ARSLAN <sinan1005@gmail.com> wrote:
Hi,

As you seen on drawing we will do fillet weld at this ring.The material grade 42CrMo4 ( SAE 4140 ).
I searched on internet it must be apply preheating which degree nearly 316ᵒ C before welding and after welding it must be apply heat thearetment ( 590  ᵒC-600  ᵒC ) and than cool down at room temperature.
Now i am looking an electrode for this material.
At enclosed i added speciality for this material.Could you advice me an electrode for this material?Which electrode?

Hub.png

--
Saygılarımla.
Best Regards.

Sinan ARSLAN
Mechanical Eng. 
Welding Eng.



--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
M.Shokri Arfaei
International Welding Engineer
RT, UT ASNT Level III
ERI-Metallurgy Lab. Manager
Tel: +98 21 66283693
Fax: +98 21 66283693
Mob.: +98 912 139 4023
Web: www.metallurgylab.com

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35289] Welding consumable for S355J2WP material

S355 J2 WP  is a weathering structural steel  It has better atmospheric corrosion resistance. Use E 8018 - W1/W2  Electrodes This is regular...