I think you misunderstood.
1. Weld pad plate with same material(same P.No.) to the shell/Pipe ( if your internals cover full of the inside of the sheel it may be of ring type or weld pad plate where internal are to be there) (WPS P1 to P1)
2. Proceed PWHT without SS316 internals.
3.After PWHT, weld SS316 internals to the Pad palte or ring as you welded with the shell/pipe before PWHT (WPS for P1 to P8)
Conduct NDE as applicable.
No need to do PWHT again,because you have not welded any direct to the shell after PWHT.

Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282


--- On Wed, 8/3/11, Vijay <k.vijayaraj@gmail.com> wrote:

From: Vijay <k.vijayaraj@gmail.com>
Subject: Re: [MW:12094] PWHT on ASME U Stamped Pressure Vessel with SS316 internals
To: materials-welding@googlegroups.com
Date: Wednesday, August 3, 2011, 11:37 PM

Dear Sirs,

Thanks for your inputs,

@Karthik: It is not having cladding. Yes, your are right they are worried about the chemical properties after PWHT. And it is 24" SCH80 Vessel, after PWHT again doing welding and again PWHT will be a time consuming job. So we have done the welding without any pads inside. This is our current situation.

@Budi: I will rise this point to our QC and let me check what further we can do.

@Ramin: For one vessel we have welded an internal and we carried out welding before PWHT. Now again cutting and removing is a difficult Task.

Thanks & Regards,
Vijay

On Wed, Aug 3, 2011 at 6:57 PM, Ramin Kondori <raminkondori@gmail.com> wrote:
Dear Vijay:

  • Remove internals,
  • weld an internal ring (same material as the shell) to the vessel (later you will weld internals to this ring),
  • carry out PWHT on vessel without internals and then
  • weld the internals to that internal ring...

This way, after PWHT, there has been no weld on shell (un-heat treated welds are on internal rings).

Good luck
Ramin  Kondori
   QC/Welding Engineer 
         IWE AT 0070
   



On Wed, Aug 3, 2011 at 2:59 PM, Vijay <k.vijayaraj@gmail.com> wrote:
Dear Experts,

We are in big trouble. We need your inputs for our problem which we
are facing now.

We are fabrication a pressure vessel with ASME U stamp. In that vessel
some internal of SS316 materials are to be welded. The size is 24".

My question: Can we do PWHT of Loading Temp @425 Deg. C and Soaking
Temp @610-630 Deg.C of 51 mins Soaking time.

Is there any code requirements for PWHT for SS internals???

We got approval from Client design team PWHT with internals and we
proceeded the welding also based on their confirmation.

Now, our QC is not accepted this method. We are in deep trouble.

Kindly clarify.

Thanks in advance.

Regards,
Vijay

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34919] Welder qualification certificate

Dear All     anyone can share a format for welder certificate and card format        Thanks & Best Regards Saleem manhappulath Mob:+9665...