[MW:11151] RE: 11150] Weld Repair Procedure- 25% Duplex Casting

Dear Mr. Bhandari,

 

Regarding minor repairs of Super Duplex Stainless Steel I would suggest to weld with a maximum interpass temperature of 150 °C.

 

One of my customers also manufactures Super Duplex Stainless Steel castings and as long as the part isn’t machined we prefer executing welding and afterwards perform solution heat treatment at 1130 °C followed by water quenching, but only for the full part and not local because of critical temperature areas as suggest by yourself.

 

After machining we only execute minor repairs by controlling interpass temperature with a maximum of 150 °C. In this way it’s not necessary to perform water quenching afterwards because the influence on surrounding material will be minimized. Of course manufacturer needs a qualified repair welding procedure for this because PWHT is an essential variable and testing need to include microstructure examination of HAZ and base material to ensure no precipitation takes place and/or sigma phase will be present.

 

Hope this will help you forward.

 

Met vriendelijke groeten / Best Regards

 

Herman Pieper

 

Pieper Quality Support & Inspection

Phone: +31 (0)521 380083

Fax:     +31 (0)84 7539225

Cell:     +31 (0)6 51691215

www.pieper-qsi.nl

 

Van: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] Namens Vikas Bhandari
Verzonden: woensdag 25 mei 2011 22:36
Aan: materials-welding@googlegroups.com
Onderwerp: [MW:11150] Weld Repair Procedure- 25% Duplex Casting

 

Hi

 

I have a weld procedure which the manufacturer of valves wants to use as a repair procedure for contingency purposes for 25% Super duplex casting.The procedure conducts solution annealing after welding. I think , for repair (allowing minor repair only,no  more than 25% of wall thickness , not more than 10% of total surface area), localised solution annealing (1120 C) is neither possible nor desirable (more chances to form embrittle precipitates in the surrounding region). So the best solution is to weld (which will raise to temperature greater than 1120 anyways) the repair , followed by water quenching after completion of welding.

 

Please correct me if I am deviating form the facts.

 

Secondly, the proposed WPS shall be rejected as PWHT is not carried out in minor repair of 25 Cr Castings.

 

Your prompt response in this regard would be much appreciated.

 

Best regards 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

nava said…
Hi Vikas Bandari,

For SDSS 25% Chromium steel , you should not do excavation by welding

I have implemented this procedure in Manchester and I got a positive result.

SDSS is normally high toughness material in my case ASTM A 890 gr
6A

I have got many repairs which exceeds the casting repair criteria.obviously we dont have another casting if we reject this.

So i have implemented and succeeded

The procedure as follows

Keep with 4 Good PT technicians

First you completely clean by diluted acid.

Clean througly use Hindustani labours.

Apply Water washable Dye Penetrant dwell time is 30 min

There is a small point. During the 30 minutes yo keep on apply penetrant so that the surface area should be wet during 30 min
Use a high quality camel hair brush

Once cleaned by Water, just do dry air blow on the surface. Then apply developer by low pressurised
comressor.15bar

You can get a good fine indications.

well how do you repair.??

This is the complicated task

If you gouge finsih, your quality of material will gone. you never excavate the repair by welding

Use a good quality hard Tunsten Carbide Tip globe,needle grinding wheel

Use pneumatic grinders donot use electric grinders.

Use good experience grinders to remove the repair, and do PT so again you get indiactaion.In this manner you will clear the defect.

Then before welding clean properly so that no penetrant residues are not there.clean 2 times apply developer again, heat clean apply developer.

so finally the excavated area doesnot have any penetrant residues.

Now preheat upto 125 deg C Use good qulaity Welding by approved WPS.

If you practice in this manner No PWHT required after repair
Try this you can realise

The basic idea is donot heat the material SDSS, for localised repair.

After repair if possible go for X-ray or Co-60 RT




Navaneethan.S
NDT L3

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...