Re: [MW:10839] ASME sect IX PQR thick Qualified

Raja is correct. If impact test is not required and PWHT is sub critical, the qualified base metal thickness: 5 - 30 mm, because your test coupon having T (not "t") 15 mm. The maximum qualified deposited weld metal thickness for GTAW process: 2t = 12mm.

T is thickness of material from test coupon, not thickness of weld deposited. It appears u use the deposited welding metal thk for GTAW to qualify base metal thickness range.

rgds

2011/4/24 raja sekhar <raj.inspection@gmail.com>
Hi,
 
No, The qualified thickness range will be 5mm to 30mm (If impact test is not required).
 
If you want to weld a 3mm thk, you have to qualify @ thk of less than or equal to 10mm.
 
Cheers!
 
Raj

On Sat, Apr 23, 2011 at 11:33 AM, Zakaria ghrab <zakaria.ghrab@gmail.com> wrote:
Hi all,

  We have a PQR, 15 mm Thickness, welded 6mm GTAW, 9mm SMAW.
According ASME sect IX, table QW-451.1, the Qualified Thickness "T" of base metal qualified will be 1.5 mm to 30 mm and the deposit weld thikness GTAW will be 12 mm max "2xt".
 Means if i have to weld pipe thick 3 mm i can't use this PQR, i'm right ?

--
زكرياء غراب


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...