[MW:6792] MW: 6787- RE: 6769] Any WPS for P91 Material without PWHT

 

Dear Faruk,

 

NO CODE WILL ALLOW  P-91 STEEL TO BE WELDED WITHOUT PWHT.

 

Further to the recommendations of John, I would like to add a few points. P-91 is classified as P 5B Gr2 material in ASME Sec-IX. Often in the past people thought this steel to be ā€œjust another Chrome Molyā€ steel, till the ā€œlessons were learntā€.  P-91 steel is never used in ambient temperature  or  typically  for   15psi  (very low) design pressure ranges. This  material is recommended for design and pressure ranges where any mishap (minor or major) could cause human fatalities. If you do a google search with these keywords ā€œ p-91 steel, failure,  fatalitiesā€, you will see tons of articles.

 

The attached article would provide a good general guidance on P-91 steel and understand the need for PWHT.

 

Let me know if it helps.

 

Thanks.

 

 

Pradip Goswami,P.Eng.

Welding & Metallurgical Engineer/Specialist

Ontario Power Generation Inc.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of John Henning
Sent: Monday, August 30, 2010 10:01 AM
To: materials-welding@googlegroups.com
Subject: [MW:6787] RE: 6769] Any WPS for P91 Material without PWHT

 

Not a good idea.  Not only is 91 in the as welded condition rather brittle but it has been shown to be subject to stress corrosion cracking in the presence of water (condensation, dew, rain, etc.).  You can find recommendations sprinkled throughout open literature that discuss the need to keep as welded 91 warm and dry between welding and PWHT.  (A tedious Google search should reveal at least four good references – a task left to you).  There have been several 91 failures traced back to SCC due to improper handling of 91 in the as welded condition.  Some recommendations not only restrict storage conditions but also time duration. 

 

As previously pointed out, all ASME codes require PWHT for all welded 91 without any exemptions.

 

John

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Mohamed Farook
Sent: Sunday, August 29, 2010 11:00 PM
To: materials-welding@googlegroups.com
Subject: [MW:6769] Any WPS for P91 Material without PWHT

 

Dear friends,

 

Greetings to all,

 

Please advise me if you have WPS for P91 material without PWHT….

 

PWHT is time consuming..

 

Thanks and Regards,

asfaruk

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


THIS MESSAGE IS ONLY INTENDED FOR THE USE OF THE INTENDED RECIPIENT(S) AND MAY CONTAIN INFORMATION THAT IS PRIVILEGED, PROPRIETARY AND/OR CONFIDENTIAL. If you are not the intended recipient, you are hereby notified that any review, retransmission, dissemination, distribution, copying, conversion to hard copy or other use of this communication is strictly prohibited. If you are not the intended recipient and have received this message in error, please notify me by return e-mail and delete this message from your system. Ontario Power Generation Inc.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...