Re: [MW:4389] ferrite number of duplex stainless steel weld


Dear all,

Our welding consumables intended for use in duplex stainless steels will normally give a weld metal with FN 35 -50.  The weld metal mechanical properties are strongly dependent on ferrite number. Higher ferrite numbers, > 50, gives higher tensile strength, lower elongation and maybe also lower Charpy values.

Welding with too low heat input will give a weld metal with too high FN, resulting in bad mechanical properties. Too high heat input will give too much brittle intermetallic phases. Since the ferrite is transformed into brittle intermetallic phase, the FN measured in the weld will be low..

Measurement of ferrite number in real weldment can be carried out with a precision of +/-10%, according to investigations carried out by IIW.


Best regards,


Claes Gillenius
Development Engineer, MMA. (Spec. stainless and non Fe-alloys)
Direct tel:  +46 (0)31 509315
Mobile +46 (0)707532012
Company                ESAB AB
Address                  Box 8004, 402 77  Gothenburg, Sweden
                                 Lindholmsallén 9
Company  reg number        556005-7738



pankaj.johri@in.transport.bombardier.com
Sent by: materials-welding@googlegroups.com

2010-02-26 06:15

Please respond to
materials-welding@googlegroups.com

To
materials-welding@googlegroups.com
cc
Subject
[MW:4375] ferrite number of duplex stainless steel weld






Hi,


We are welding duplex stainless steel.


To control the parameters of welding, we are measuring ferrite number of weld.


Can anybody tell us how acceptable values of ferrite numbers are decided.



Regards,

Pankaj



Please consider the environment before you print / Merci de penser à l'environnement avant d'imprimer

_______________________________________________________________________________________________________________
This e-mail communication (and any attachment/s) may contain confidential or privileged information and is intended only for the individual(s) or entity named above and to others who have been specifically authorized to receive it. If you are not the intended recipient, please do not read, copy, use or disclose the contents of this communication to others. Please notify the sender that you have received this e-mail in error by reply e-mail, and delete the e-mail subsequently. Please note that in order to protect the security of our information systems an AntiSPAM solution is in use and will browse through incoming emails.
Thank you.
_________________________________________________________________________________________________________________

Ce message (ainsi que le(s) fichier(s)), transmis par courriel, peut contenir des renseignements confidentiels ou protégés et est destiné à l'usage exclusif du destinataire ci-dessus. Toute autre personne est, par les présentes, avisée qu'il est strictement interdit de le diffuser, le distribuer ou le reproduire. Si vous l'avez reçu par inadvertance, veuillez nous en aviser et détruire ce message. Veuillez prendre note qu'une solution antipollupostage (AntiSPAM) est utilisée afin d'assurer la sécurité de nos systèmes d'information et qu'elle furètera les courriels entrants.
Merci.
_________________________________________________________________________________________________________________

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


This communication and any files transmitted with it contain information which is confidential and which may also be privileged. It is for the exclusive use of the intended recipient(s). If you are not the intended recipient(s), please note that any disclosure, copying, printing or use whatsoever of this communication or the information contained in it is strictly prohibited. If you have received this communication in error, please notify us by e-mail or by telephone as above and then delete the e-mail together with any copies of it. ESAB does not accept liability for the integrity of this message or for any changes, which may occur in transmission due to network, machine or software failure or manufacture or operator error. Although this communication and any files transmitted with it are believed to be free of any virus or any other defect which might affect any computer or IT system into which they are received and opened, it is the responsibility of the recipient to ensure that they are virus free and no responsibility will be accepted by ESAB for any loss or damage arising in any way from receipt or use thereof.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...