Monday, February 15, 2010

Re: [MW:4316] IMPACT TEST IN LOWER TEMPERATURE

E8018 C1
it has nickel which will give high impact values even at -50 degree.

On Mon, Feb 15, 2010 at 12:18 PM, Sudhakar K <sudhaakar.k@gmail.com> wrote:
Hi Ali,
 
As the impact temp is -40 deg C, its 50-50 chances are there, where as if you use E 7016 G in place of E 7018-1, definitely you will get the required values.
Let us know the outcome.
 
rgds
Sudhakar
On Fri, Feb 12, 2010 at 3:01 PM, Ali Asghari <asghariali@rocketmail.com> wrote:
hi all
i have a pwps that the grade of base metal is S355K2G3Z35.now contractor want to test this pwps in -40.
the description of pwps:1-root pass 3.2 dia 7016-1(WITH IMPORTANT ELEMENTS: C=.04,MN=1.10,NI=.02,NB=.01,V=.01,CU=.01)
OTHER passes deposited with 7018-1(WITH IMPORTANT ELEMENTS:C=.08,MN=1.42,NI=.02,NB=.01,V=.01,CU=.05)with different dia:3.2,4,5
does any body have recommendation to get enough toughness(36 kj) in this temp?
regards

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...