Hello Mr. Kannan,
Yes you need an impact test for A106 gr.B pipe , of 4'' XXS xch... thik. 17.12 mm at MDMT -29 deg.C.
As per ASME 31.3 , chart 323.2.2A and Table 323.2.2A,, the limiting thickness for MDMT -29 deg C is 12.7 mm for A106 gr. B pipe.
It is advisable to use A333 Gr. 6 material for your situation
Kind regards
Rahul Pisat
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of rajagopal kannan
Sent: zondag 3 januari 2010 12:39
To: materials-welding@googlegroups.com
Subject: Re: [MW:3949] Re: Usage of A106 gr. B pipe
Dear Members,
Sorry for not mentioning the design pressure.
It is 5000 PSI. Is it required for the A 106 Gr. B material to undergo impact testing at -29 deg.c, if the MDMT is -29 deg.c and the thickness is 17.12mm Thick.
Thanks,
K.Rajagopal
On Sun, Jan 3, 2010 at 2:30 PM, israr <ahmedisrar.nm@gmail.com> wrote:
Yes U can use.
For more detail Ref Chart Tempreture Vs thickness Ref UCS 66 of asme
section VIII Div.1
Ragards
Israr Ahmed
KSA
+966530417332
On Jan 2, 9:10 am, rajagopal kannan <rajagopal.kan...@gmail.com>
wrote:
> Dear Members,
> Can you please advise whether A 106 Gr. B 4" sch. XXS pipe, be used for MDMT
> -29 Deg.C, as per B 31.3?
> Thanks and Regards,
> K.Rajagopal
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
____________________________________________________________________________
This email has been scanned for Viruses and Spam. For more information
please contact your local Business Unit Information Security representative.
____________________________________________________________________________
No comments:
Post a Comment