Monday, October 12, 2009

[MW:3493] RE: 3490] Welding of Sa-335 to SA-106

Jimmy

Per ASME Section IX

Provided impacts are not required (!) by the design code or customer,
one can use a P4-to-P4 procedure qualification (PQR) to write a P4-to-P1
welding procedure. All other essential variables must be the same,
which generally means that your weld metal will match the higher alloy
(in this case 1-1/4Cr 1/2Mo).

This is covered in Sc IX, QW-424.1:

"Base metal(s) used for procedure qualification coupon . . . One metal
from P-No.4 to any metal from P-No 4"
"Base metals qualified . . . Any P- or S-No.4 metal to any metal
assigned P- or S-No. 4, 3, 1"

Again this is valid only if impacts are NOT required which invokes the
supplementary essential variables.

John

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Jimmy Nielsen
Sent: Monday, October 12, 2009 3:50 AM
To: Materials & Welding
Subject: [MW:3490] Welding of Sa-335 to SA-106


Hello Gents

Can sombody help me with a answar regarding welding of Sa-335 to SA-106.

I have a PQR covering material 335-P11 to 335-P11( P4) Can I use it for
welding of P-no 4 to P-no 1

Regard, jimmy

--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...