[MW:1223] Re: FCAW --- UT / RT ???

I HAVE FEW QUESTIONS TO ASK BEFORE COMMENTING ANYTHING ON THIS.
1. WHAT IS THE INCLUDED ANGLE OF THE GROOVE?
2. WHAT IS THE ESO YOU ARE TAKING AND WHAT IS RECOMMENDED BY
MANUFACTURER.
3. WHAT ARE THE WELDING PARAMETERS
4. AT WHAT LOCATION, WITHIN THE GROOVE, YOU ARE GETTING LOF/
POROSITIES?
5. BEAD DEPOSITION IS STRINGER OR WELDER IS EMPLOYING WEAVING
TECHNIQUE?

PLEASE CLARIFY.

SANJAY JAIN


On Sep 19, 10:42 pm, "PREM SHANKARDUTT NAUTIYAL"
<prem_nauti...@rediffmail.com> wrote:
>   
> Dear Friends
>
> We are presently using FCAW process(E71T-1) for welding SA516Gr.70 material in 3G and 1G. The joint calls for 100% RT and UT. The thickness is 70mm with double V.
> But everytime we get repair in the weld like slag, LOF,porosities..
>
> So my basic question is can FCAW be used to weld RT and UT joints??
> If yes what is the correct procedure / precautions to be followed..
>
> Regards
>
> Prem Nautiyal
>
> PREM S NAUTIYAL
> CELL : 9820313278

--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .