-----Original Message-----
From: PEMMARAJU RAGHAVENDRA [mailto:rpe@hzw.ltindia.com]
Sent: Tuesday, October 07, 2008 5:30 AM
To: Bathula Raghuram (Mumbai - PIPING); skumarswami@yahoo.co.in
Subject: Re: [MW:1177] Radiography of tube to tubesheet welds


We have done extensive RT of such joints in the past.
We have adopted the back radiation technique in which the source shall be moving from the front side of the joint. We have used the roli camera without guide tube and only the cranking unit wire coupled with source pigtail shall be used.The film used was of AGFA D4 with a special type of cassette with a hole at the centre.Vide this hole on the film cassette, the source enters into its position in case of back radiation technique.
It is preferred to use low curie source of Ir-192 of the order 3 to 4Ci.
Refer the attached word file for the source and film setup.

Instead of Gamma rays, you may use micro-focus X ray machine with hooded anode target which was developed by Sasol.


regards,
RPE


Larsen & Toubro Limited
www.larsentoubro.com

This Email may contain confidential or privileged information for the intended recipient (s) If you are not the intended recipient, please do not use or disseminate the information, notify the sender and delete it from your system.


From: Bathula Raghuram (Mumbai - PIPING) <R.Bathula@ticb.com>
Subject: [MW:1177] Radiography of tube to tubesheet welds
To: "Materials-Welding (E-mail)" <materials-welding@googlegroups.com>
Date: Wednesday, 1 October, 2008, 1:48 PM

Can anybody has experience with performance of RT on tube to tubesheet welds,
please share details for both techniques (i.e. back radiation and forward
radiation), equipment literature if any for this type RT.

--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...