about actual welding parameter such as Heat Imput and Interpass Temperature
as well as details about thickness and number of weld runs in your weld.
In general you have to keep your heat imput below 1.5 kJ/mm and your
interpass temperature below 150°C and in some cases even below 125°C.
Especially this max. 1.5 kJ/mm is difficult for GTAW process.
Met vriendelijke groeten / Best Regards
Herman Pieper
Pieper Quality Support & Inspection
Phone: +31 (0)521 380083
Fax: +31 (0)84 7539225
Cell: +31 (0)6 51691215
www.pieper-qsi.nl
-----Oorspronkelijk bericht-----
Van: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] Namens biju
Verzonden: maandag 18 april 2011 19:59
Aan: Materials & Welding
Onderwerp: [MW:10727] welding of super duplex stain less steel and critical
pitting temp.
In our project during procedure qualification for super duplex stain
less steel we are not able to achieve the specified critical pitting
temperature.Welding conditions are
GTAW
ER2594
88%Argon+2%Nitrogen shielding gas
What we have to do to acieve the CPT
PLEASE REPLY
REGARDS
BIJU
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and
meant for educational purposes only, Users must take their own decisions
w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Comments