Thursday, November 5, 2020

Re: [MW:31712] RE: 31689] Cast iron to mild steel

Dear Sir,

Thank you very much for your valuable advice on consumable selection. 

Appreciate it. 

On Tue, 3 Nov 2020 at 12:23, <pgoswami@rogers.com> wrote:

Hello Pravin

Cast iron is one of the difficult metals to weld. Grey cast irons are weldable subject to the original manufacturing process and grades involved. White cast irons are Unwedable. It's important to know what's the grade involved. Welding cast iron is typically a repair weld. Qualifying ASME Sec-IX procedures as like new fabrication  is quite difficult. One may have to settle with reduced angle of bending in "Guided Bend Test". Some resources are attached for guidance.

Usually E-Ni-CI (99% Nickel) or ENiFe-CI(55%Ni) SMAW electrodes or GMAW fillers of equivalent composition are available for the consumable manufacturers.

If you want to know the subject well, get hold of this AWS publication.

Thanks.

 

P.Goswami.P.Eng, IWE.

Independent  & Consulting Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@rogers.com,pradip.goswami@gmail.com

Cell/Whasapp:1-905-9793232

 

https://www.lincolnelectric.com/en-us/support/welding-how-to/Pages/welding-cast-iron-detail.aspx

 

 

From: materials-welding@googlegroups.com <materials-welding@googlegroups.com> On Behalf Of Pravin Poornachandran
Sent: November 2, 2020 9:29 PM
To: 'Bijay' via Materials & Welding <materials-welding@googlegroups.com>
Subject: [MW:31689] Cast iron to mild steel

 

Dear Expert, 

 

Good day.

 

I have to weld cast iron to mild steel.

What would be the suitable filler rod to use? 

 

Also is there any specific parameter or welding condition I have to follow since cast iron is difficult to weld. 

 

Example any specific heat treatment or post heating before welding? 

 

Kindly advice.

 

Best regards,

Pravin 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADDyn7eaVq1UvD%2BgBxN8BiwjvxLoa4MSduXQisFPpOo4fRfStA%40mail.gmail.com.


Virus-free. www.avg.com

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/!%26!AAAAAAAAAAAuAAAAAAAAABVPzeizzeRJsiPziIE5jXQBAMO2jhD3dRHOtM0AqgC7tuYAAAAAAA4AABAAAACDR34A1Ms0SqFI15CaIAt7AQAAAAA%3D%40rogers.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADDyn7eeWpcpentZ7m7pM9GH7j29%3DNtcwtLS87Qm1VQVJQrEnA%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...