Skip to main content

Re: Re: [MW:28669] PQR testing with RT & UT

Yes, QW-355 is clear, GMAW / FCAW.


Regards,
Mohamed Muneeb Mahaboob
CSWIP 3.2-89247/2 
ASNT-NDT-L2-RTFI-RT-UT-MT-PT.
SAP#:70021650 APs:JAPID, QCS & QCI.
E muneebslsa@gmail.com M +91-636-955-7189

(6:59) He has the keys to the realm that lies beyond the reach of human perception; none knows them but He. And He knows what is on the land and in the sea; there is not a leaf which falls that He does not know about and there is not a grain in the darkness of the earth or anything green or dry which has not been recorded in a Clear Book.

 
Date: 2018-11-23 08:38
Subject: Re: [MW:28660] PQR testing with RT & UT
Hi,
Please refer Table QW-355, it clearly specified as FCAW included.




Thanks& Regards,

 

(Karthik)

Karthikeyan.S

QA/QC Manager
Agon Pacific Co.,Ltd.
M: +66-655-174-397, +66-892-512-282

E-mail : karthik6684@yahoo.com



On Thursday, November 22, 2018, 5:27:26 PM GMT+7, Saif <saif.jesan01@gmail.com> wrote:



Hi,
I have one clarification about QW-304. There mention Volumetric test can be perform for WPQR. But process there mention FCAW are not in this. So, what can i do for FCAW process? Is there any code reference that GMAW & FCAW are considering same process?

Thank You
Saif Uddin
Quality Manager
NDE Steel Structure Limited.



On Saturday, 16 July 2011 10:46:02 UTC+6, Karthik wrote:
Hi,
There is no such specification in ASME Sec.IX. As per ASME Sec.IX mechanical tests only to be conducted for WPS/PQR regardless of Process(es). But most of the companies do RT or UT before doing mechanical tests to confirm that there is no defect.But this is not a Code requirement.

QW-202 Type of Tests Required

QW-202.1 Mechanical Tests. The type and number of

test specimens that shall be tested to qualify a groove weld

procedure are given in QW-451, and shall be removed in

a manner similar to that shown in QW-463. If any test

specimen required by QW-451 fails to meet the applicable

acceptance criteria, the test coupon shall be considered as

failed.


 
Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282


--- On Fri, 7/15/11, ABHISHEK GHOSH <ghoshabh...@gmail.com> wrote:

From: ABHISHEK GHOSH <ghoshabh...@gmail.com>
Subject: [MW:11740] PQR testing with RT & UT
To: material...@ googlegroups.com
Date: Friday, July 15, 2011, 10:57 PM

Dear Experts, 

Why UT along with RT is performed while qualifying a procedure with FCAW welding, At which clause in ASME 9 it is mentioned that UT & RT both has to be performed ?? 

With regards. 

AG

--
ABHISHEK GHOSH
FAHAHEEL, KUWAIT
MOB: (00)965-65772043

--
To post to this group, send email to material...@ googlegroups.com
To unsubscribe from this group, send email to materials-weld...@ googlegroups.com
For more options, visit this group's bolg at http://materials-welding. blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...