Skip to main content

RE: [MW:25351] LTCS PQR

Hi buddy!!!

Since your joint is between P.No 1-Gr No 1 (A333-Gr6) and P.No1-Gr No2 (A350 LF2) and impact test is mandatory (cause Gr No to be essential variable) so your PQR shall joint between P.No 1-Gr No 1 & P.No1-Gr No2. I think most available material to meet above-mentioned criteria is SA-516Gr70 to SA-516Gr60.

your quarries;
a) If you do not have other thicknesses so thickness 10mm is so enough!.
b)Yes.
c)GTAW filler; ER-80SNi(if NACEMR0175/ISO15156 is not applicable)/SMAW filler: E7018-1.

Regards,
Himan Nikdin


Date: Wed, 7 Sep 2016 22:21:03 -0700
From: mustaqnk@gmail.com
To: materials-welding@googlegroups.com
Subject: [MW:25350] LTCS PQR

Dear Experts 

I am new for this job please help me 

for PQR of LTCS

1) required thickness min is 6.35mm &  dia is 12 inch

2) design press = 20kg/cm2
    design temp  = -45.6/37.8 degreee celcius
     op press      = 20 max
     op temp       = -40 degree celcius

3)  material is pipe - A 333 GR 6(P1 &G1) and flange - A350 GR LF2 RF

4) service is LPG plant- Relief and blow down

now please suggest me 
 a) what is is the size of the test coupon can be selected(dia with schd) where can i find the exact length of weld required to carry out mechanical testing for this PQR?
 b) is it possible to carry out the PQR for pipe to flange joint 
 c) what consumable can be selected for this if GTAW & SMAW ?
 

Regards
AHMAD

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1dff4f26-85ba-4a9d-a731-d037ac27bea3%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...