Re: [MW:25201] PQR Qualification.

correct, you need a new PQR

2016-08-05 17:30 GMT+03:00 r.vroom <r.vroom@gmail.com>:
All,

Please advice me in the following.
ASME IX :2013
Weld coupon base material P8 (ASTM A240 TP 316) to P1 (S333 Gr. 6)
FCAW: Filler metal Bohler CN 23/12 Mo PW-FD (E309LMoT1-4)

Does this PQR qualify a weld joint P8 (ASTM A240 TP 304) to P8 (ASTM A240 TP 304)
by changing filler metal into E308LT1-1 for both F No. 6 and A No. 8

Follow Table QW 255 Ø P-number qualified article 403.11 -> article 424.1 I should say no, but am I right ????


Diameter and thickness are in range.

Thank you.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/83ce3674-8b7a-42d2-b8f6-98aa0cdb35db%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40AemTcJSjQ%2BWBgMJVLdj3CaUHUN1xUYO7Wg9XYp5uygoA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35354] Cast-iron welding

1. Preheat joint area(other area, cover with mineral wool). 2. ENiCi or ENiFe-CI. 3. stringer bead. 4. peening is to be done on weldmetal im...