Monday, November 2, 2015

Re: [MW:23843] Tensile testing

Dear all,

In order to get the 0.2% yield or proof stress, in the load vs extension curve take a point on x-axis at 0.2% of gauge length ( if 50 is GL then this point is  0.1mm on the x-axis ie along the extension). From this point draw a parallel line to the curve obtained by tensile test. This line would meet the curve at a point. Load corresponding to this is the 0.2% proof load and the stress based on this will give 0.2% Proof stress. Since some alloy steel unlike mild steel does not have a specific point of yield, this method is suggested for estimating the yield strength allowing a permanent yield of 0.2%. Software will have this but you have to verify that 0.2% of GL marked is taken for getting the value.

With warm regards

Mohan Ananthanarayanan
DGM QC VSSC


On Fri, 30 Oct 2015 20:28:50 +0400, Harish Kannepalli wrote
> Did u use extensometer or not?
> You have to construct 0.2% offset on the strain axis and get the 0.2% yield strength. Probably ur software would have that option!
>
> 2015-10-29 19:13 GMT+04:00 Padmasanker S <padmasanker87@gmail.com>:
>

> Dear all,
> Please refer to attached stress -strain graph obtained during tensile testing of SA 106 Gr B pipe.
> While performing tensile testing of SA 106 pipes for Div 1 vessels ,we were not getting yield point even though required tensile strength is obtained.
> The specimen were taken in both  transverse and longitudinal direction from half thickness.
> Kindly share your experience  in finding the root cause..
> Please inform if any further details is required for clarity.
>
> Best regards,
> Padmasanker,
> Quality coordinator,
> Bilfal heavy industries ltd.
> --
> You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
> To post to this group, send email to materials-welding@googlegroups.com.
> Visit this group at http://groups.google.com/group/materials-welding.
> To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKDH8Gq%2BubEPKfFeaLTemr8ekcAO-KuOaddmKfrjwLEoDahXYQ%40mail.gmail.com.
> For more options, visit https://groups.google.com/d/optout.
>

>

>
> --
>
> Regards,
> Mr. Harish.
> --
> You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
> To post to this group, send email to materials-welding@googlegroups.com.
> Visit this group at http://groups.google.com/group/materials-welding.
> To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAE4SttGRCQDyJMX957rJZT4Jsu5ZnaT88gLACZwcxz6WLY1dOg%40mail.gmail.com.
> For more options, visit https://groups.google.com/d/optout.


No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...