Hi

Typical methods for PMI are XRF and OES (both portable methods). 
XRF is more qualitative than OES and could not be used for C, S & P measurement (Its weak point is measuring light elements)
Portable OES (with spark method) has ability to measure C more accurate compare with XRF and less accurate compare with Stationary OES, but has same situation for S & P.

My experience says, after calculation of carbon equivalent if you got a number near the criteria ( about 0.01 or 0.02% below or above it) do not rely on portable OES results.

Regards

On Fri, Sep 11, 2015 at 4:59 PM, Ramesh Kumar <rameshkumarkbs1@gmail.com> wrote:
Dear Jay

We cant replace chemical test with PMI.
We cant get the carbon equivalent with the help of PMI.
regards
KBS RAMESH KUMAR


On Fri, Sep 11, 2015 at 3:38 PM, Jay Poojary <jayogini@gmail.com> wrote:

Dear Experts,

Is PMI replacement for chemical test. With PMI can Carbon equivalent be known?

Kindly advise
Thank you
Jay poojary

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAAcO%3DyS%3Dq8MEExqfBwbXHby7yOZaqP8Y%2B18DDHj%3DJY8DQrM_rw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPTccU9t4ndGDkDbMFWeuRUP%2BPhFL1MTK63kir_Fg1sDufT8WQ%40mail.gmail.com.

For more options, visit https://groups.google.com/d/optout.



--
M. Shokri Arfaei
ISA-ISTS - Metallurgy Lab. Manager
ASNT NDT Level III
International Welding Engineer

Tel.: +98 21 66282127
Fax: +98 21 66282779
Mob.:+98 912 1394023




--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAC8uMtv2XK3SaN%3Dr4%2B72ckSGqvp6i9zKm0ML6raCZfZ%3DBdM-cA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35354] Cast-iron welding

1. Preheat joint area(other area, cover with mineral wool). 2. ENiCi or ENiFe-CI. 3. stringer bead. 4. peening is to be done on weldmetal im...