ASME A Numbers 
These refer to the chemical analysis of the deposited weld and not the parent material.  They only apply to welding procedures in steel materials.
 

A1

Plain unalloyed carbon manganese steels.

A2 to A4

Low alloy steels containing Moly and Chrome Moly

A8

Austenitic stainless steels such as type 316.

 

ASME F Numbers 
 

F Number

General Description

1

Heavy rutile coated iron powder elctrodes :- A5.1 : E7024

2

Most Rutile consumables such as :- A5.1 : E6013

3

Cellulosic electrodes such as :- A5.1 : E6011

4

Basic coated electrodes such as : A5.1 : E7016 and E7018

5

High alloy austenitic stainless steel and duplex :- A5.4 : E316L-16

6

Any steel solid or cored wire (with flux or metal)

2X

Alluminium and its alloys

3X

Copper and its alloys

4X

Nickel alloys

5X

Titanium

6X

Zirconium

7X

Hard Facing Overlay

Note:- X represents any number 0 to 9



On Fri, Jan 24, 2014 at 5:45 PM, Binoy Lonappan <binoypl3@gmail.com> wrote:
Dear All ,

Can anyone explain the ways or steps for selecting electrodes for various process,

A no. F no and composition where to refer these things 

--
With Regards
Binoy Lonappan
+91-9645100560
QAC Engineer
TECCL




--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.



--

 Best Regards,

 Raghib Ali
QA/QC Inspector

Mobile: +971 55 5865648


Lamprell Energy Ltd
PO Box 42149, Port Khalid, Sharjah, United Arab Emirates.
Tel: +971 6 528 5345 | Fax: +971 6 528 5820


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...