Skip to main content

Re: [MW:16391] Vacuum Packed LH Electrodes

Mr. Abhisekh,

" After opening packet at the start of the days work , is it necessary to transfer a pack of  electrodes to a portable quiver for holding 
at temp 100 deg C to prevent further moisture pick up ? or it is not required as manufacturer says that after opening up to 9 hrs it can be used at 80% / 27 deg C .

Electrodes rebaking cycle depends upon which factors? Some client specifies recycling 1 time  , some 2 times ... [ As per BIS 13851:1993 , ( R 2006) - Storage & redrying of coverd electrodes  before use recommendations- 3 times ] "

Answer:
The very purpose of using  E 7018-1 H4 type Vacuum packed Electrodes is to avoid re-backing, as the H2 level is 
<4 ml /100 grams of weld and can be used straight after opening the pack. 

When not used  after  breaking the seal and considerable gap of time, re-baking is to be done, as the electrodes would 
have picked up  moisture by then, due to its exposure to humid conditions.

Without H-4 designation, all low Hydrogen type electrodes may have > 10 ml  & < 15 ml of H2 per 100 grams of weld and compulsory re-drying has to be done to reduce the H2 content to <10 ml. by holding them at 300 deg. C for 2 hrs 
in the ovens.

The electrodes are held in Holding oven (if required) at 100-150 deg.C,  if backed in large quantity and to avoid repeated 
re-baking (re-cycling) and damage to flux coating if unused.

Welders are supposed to use portable (kept at 100 deg. C or so) for actual welding. These ovens also know as re-fill ovens
as the electrodes are refilled after every 2 hrs welding work or less.  

Sridhar.


From: ABHISHEK GHOSH <ghoshabhishekmech@gmail.com>
To: materials-welding@googlegroups.com
Sent: Sunday, 30 December 2012 11:17 AM
Subject: [MW:16383] Vacuum Packed LH Electrodes

Dear Experts, 

We are using E 7018-1 H4 Vacuum packed Electrodes for our project. ( Refer attachments ) , where manufacturer recommendations is mentioned as : 
HD [ ml/100g] : at opening time : <5 
Working time after opening : 9h at 80% RH / 27 deg C 
After this period rebaking : 2h/340-360 deg C 
Brand : Supercito VP Medium ,Oerlikon , Air Liquide Wedling France. 
Weather Condition at site : 78- 80 % Humidity , Temp 26-30 Deg C. 

My question is :
 After opening packet at the start of the days work , is it necessary to transfer a pack of  electrodes to a portable quiver for holding at temp 100 deg C to prevent further moisture pick up ? or it is not required as manufacturer says that after opening up to 9 hrs it can be used at 80% / 27 deg C . 

  • Electrodes re-baking cycle depends upon which factors? Some client specifies recycling 1 time  , some 2 times ... [ As per BIS 13851:1993 , ( R 2006) - Storage & redrying of coverd electrodes  before use recommendations- 3 times ] 

Please clarify . 

Thanks & regards. 

Abhishek Ghosh 
Indonesia 
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 


Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...