Sunday, December 23, 2012

[MW:16308] RE: 16305] Welding for cast iron repair

Dudy,

By and large Gray and nodular cast irons are weldable, NOT THE WHITE CAST IRONS.

The  recommended  electrodes for welding these  two mentioned varieties are :- Pure -99% Nickel type, and 55 -45 Ni-Fe type . By and large a sustained preheat & interpass temperature control  would be recommended - of the range 150-250 Deg C. Note cast iron can be only repaired,do not expect to have very high level of  metallurgical integrity from this repair.

Please find the links below as useful guidelines.

Thanks

Pradip Goswami,P.Eng.IWE
Welding & Metallurgical Specialist
Ontario, Canada.
Email-pgoswami@sympatico.ca,
pgoswami@quickclic.net
 
 
 

-----Original Message-----
From: materials-welding@googlegroups.com [
mailto:materials-welding@googlegroups.com] On Behalf Of Dudy Firdaus
Sent: Sunday, December 23, 2012 1:50 AM
To: materials-welding@googlegroups.com
Subject: [MW:16305] Welding for cast iron repair

Dear Experts,

Could you share me the best experiences regarding with welding for cast iron repair?
What in best process of welding and spec of the electrodes?

Highly appreciated for your help.
Thanks.

Kind Regards,

Dudy Firdaus
m: +62 85859020475 ; +62 81217149000
e: dudy.pfirdaus@yahoo.com.au
www.linkedin.com/pub/dudy-firdaus/1a/44/558

Sent from my Private BlackBerry®

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...