Skip to main content

Re: [MW:15147] Problem about Positive material Identification (PMI)

Dear Mr. Jubair,
                         Normally there is dilution of electrode chemistry in the weld. As a demonstration to your client, weld a pad of 200x200mm on T91 pipe with the same electrode and check chemistry at different heights from fusion line (FL+3, FL+8, etc). So you can accept this weld upto a defined dilution (say 10%).

2012/8/28 kulandaivel__subramani_ <subramak@batelco.com.bh>
Check with another PMI equipment preferably using XRF equipment.

On Tue, 28 Aug 2012 13:55:05 +0530
 mohamed jubair <kmd.jubair@gmail.com> wrote:
Dear all,****

** **


In our  boiler one major problem occurred in Positive
Material
Identification(PMI) test [Spectrum test].  ****

** **

Description****

Reheater finishing outlet(RHFO) coil****

Material****

T91****

Size****

ø 63 x 4****

Process****

GTAW only****

Filler wire****

ER 90S B9****

Filler wire Manufacturer****

D & H Secheron****

Preheating °C****

185****

Rate of Heating  °C****

100/hr****

Interpass temp  °C****

190****

Post heating  °C****

100****

PWHT  °C****

750****

Soaking Time****

90 minutes****

****


Around 800 joints welded in the above approved procedure
only. Filler wire,
header stub, RHFO coil, weld metal undergone PMI test
separately and all
show positive material results as T91 except weld metal.
Weld metal shows
the Chromium content only  as (4-7%){Reqd is 8-10.5%}.
We can't find how
it happened? Our Chinese consultant told to cut and
reweld all the joints.
But our contractor argued that we followed approved
procedure and used
approved vendor's consumable only. Please give a
solution. Here I have
attached one preheating cum PWHT chart of RHFO
joints(for 11 joints,5
thermocouples,1 recorder).All 800 joints are not checked
yet. Only 40
joints checked and all 40 weld metals shown low Cr
Content.**



Please go through the below readings of one RHFO
joint.****

*Description*

*Filler wire*

*Header stub*

*Weld metal*

*RHFO coil*

Alloy****

T91****

T91****

A-2****

T91****

Cr****

8.94****

8.34****

5.19****

8.68****

Mo****

0.96****

0.90****

0.93****

0.92****

V****

0.17****

0.17****

0.08****

0.19****

Ti****

0.07****

0.10****

0.04****

0.03****

Mn****

0.60****

0.40****

0.54****

0.63****

Fe****

87.81****

88.11****

90.86****

87.61****

Ni****

0.12****

0.33****

0.20****

0.38****

Cu****

0.02****

0.16****

0.20****

0.16****

Nb****

0.09****

0.08****

0.03****

0.04****

W****

0.15****

****

0.00****

****

** **

Waiting for your valuable suggestions.

Thanks & Regards
K Mohamed Jubair

--
To post to this group, send email to
materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members
personel views and meant for educational purposes only,
Users must take their own decisions w.r.t. applicable
code/standard/contract documents.



--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.





--
regards,
Harish.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...